Difference between revisions of "Lithography Recipes"
Jump to navigation
Jump to search
(deleted erroneous columns) |
(→Photolithography Recipes: correcting row colors) |
||
Line 59: | Line 59: | ||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
+ | |- |
||
− | |- bgcolor="#D0E7FF" |
||
! colspan="7" height="45" |<div style="font-size: 150%;">Photolithography Recipes</div> |
! colspan="7" height="45" |<div style="font-size: 150%;">Photolithography Recipes</div> |
||
+ | |- |
||
− | |- bgcolor="#D0E7FF" |
||
− | |<!-- INTENTIONALLY BLANK -- |
+ | | bgcolor="#EAECF0" | <!-- INTENTIONALLY BLANK --> |
− | ! colspan="2" |
+ | ! colspan="2" align="center" |'''[[Contact Alignment Recipes|<big>Contact Aligner Recipes</big>]]''' |
− | ! colspan="3" |
+ | ! colspan="3" align="center" |'''[[Stepper Recipes|<big>Stepper Recipes</big>]]''' |
− | ! |
+ | ! align="center" |Other |
|- |
|- |
||
! width="150" bgcolor="#D0E7FF" align="center" |'''Positive Resists''' |
! width="150" bgcolor="#D0E7FF" align="center" |'''Positive Resists''' |
||
{{LithRecipe Table}} |
{{LithRecipe Table}} |
||
+ | |- bgcolor="EEFFFF" <!-- This is the Row color: lightblue --> |
||
− | |- |
||
| bgcolor="#D0E7FF" align="center" |AZ4110 |
| bgcolor="#D0E7FF" align="center" |AZ4110 |
||
− | + | |{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
|
− | + | |{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
|
+ | |A |
||
− | | bgcolor="EEFFFF" |A |
||
+ | |A |
||
− | | bgcolor="EEFFFF" |A |
||
− | | bgcolor="EEFFFF" | |
||
| |
| |
||
− | | |
+ | | |
+ | |- <!-- This is a White row color --> |
||
| bgcolor="#D0E7FF" align="center" |AZ4210 |
| bgcolor="#D0E7FF" align="center" |AZ4210 |
||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
||
Line 84: | Line 84: | ||
|A |
|A |
||
|A |
|A |
||
− | |<br> |
||
| |
| |
||
− | | |
+ | | |
+ | |- bgcolor="EEFFFF" |
||
| bgcolor="#D0E7FF" align="center" |AZ4330RS |
| bgcolor="#D0E7FF" align="center" |AZ4330RS |
||
− | + | |{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
|
− | + | |{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
|
+ | |A |
||
− | | bgcolor="EEFFFF" |A |
||
+ | |A |
||
− | | bgcolor="EEFFFF" |A |
||
+ | | |
||
− | | bgcolor="EEFFFF" | |
||
| |
| |
||
|- |
|- |
||
+ | | bgcolor="#D0E7FF" align="center" |AZ4620 |
||
− | |AZ4620 |
||
| |
| |
||
| |
| |
||
Line 102: | Line 102: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="EEFFFF" |
||
+ | | bgcolor="#D0E7FF" align="center" |OCG 825-35CS |
||
+ | | A |
||
+ | | A |
||
+ | | A |
||
+ | | A |
||
+ | | |
||
+ | | |
||
|- |
|- |
||
− | | bgcolor="#D0E7FF" align="center" | |
+ | | bgcolor="#D0E7FF" align="center" |SPR 950-0.8 |
|A |
|A |
||
|A |
|A |
||
|A |
|A |
||
|A |
|A |
||
− | |<br> |
||
| |
| |
||
− | |- |
||
− | | bgcolor="#D0E7FF" align="center" |SPR 950-0.8 |
||
− | | bgcolor="EEFFFF" |A |
||
− | | bgcolor="EEFFFF" |A |
||
− | | bgcolor="EEFFFF" |A |
||
− | | bgcolor="EEFFFF" |A |
||
− | | bgcolor="EEFFFF" | |
||
| |
| |
||
+ | |- bgcolor="EEFFFF" |
||
− | |- |
||
| bgcolor="#D0E7FF" align="center" |SPR 955 CM-0.9 |
| bgcolor="#D0E7FF" align="center" |SPR 955 CM-0.9 |
||
|A |
|A |
||
Line 124: | Line 124: | ||
|{{rl|Stepper Recipes|Positive Resist (GCA 6300)}} |
|{{rl|Stepper Recipes|Positive Resist (GCA 6300)}} |
||
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} |
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} |
||
+ | | |
||
− | |<br> |
||
| |
| |
||
|- |
|- |
||
| bgcolor="#D0E7FF" align="center" |SPR 955 CM-1.8 |
| bgcolor="#D0E7FF" align="center" |SPR 955 CM-1.8 |
||
+ | |A |
||
− | | bgcolor="EEFFFF" |A |
||
+ | |A |
||
− | | bgcolor="EEFFFF" |A |
||
− | + | |{{rl|Stepper Recipes|Positive Resist (GCA 6300)}} |
|
− | + | |{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} |
|
− | | bgcolor="EEFFFF" | |
||
| |
| |
||
− | | |
+ | | |
+ | |- bgcolor="EEFFFF" |
||
| bgcolor="#D0E7FF" align="center" |SPR 220-3.0 |
| bgcolor="#D0E7FF" align="center" |SPR 220-3.0 |
||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
||
Line 140: | Line 140: | ||
|{{rl|Stepper Recipes|Positive Resist (GCA 6300)}} |
|{{rl|Stepper Recipes|Positive Resist (GCA 6300)}} |
||
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} |
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} |
||
+ | | |
||
− | |<br> |
||
| |
| |
||
|- |
|- |
||
| bgcolor="#D0E7FF" align="center" |SPR 220-7.0 |
| bgcolor="#D0E7FF" align="center" |SPR 220-7.0 |
||
− | + | |{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
|
− | + | |{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
|
− | + | |{{rl|Stepper Recipes|Positive Resist (GCA 6300)}} |
|
− | + | |{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} |
|
− | | bgcolor="EEFFFF" | |
||
| |
| |
||
− | | |
+ | | |
+ | |- bgcolor="EEFFFF" |
||
| bgcolor="#D0E7FF" align="center" |THMR-IP3600 HP D |
| bgcolor="#D0E7FF" align="center" |THMR-IP3600 HP D |
||
+ | | |
||
− | |<br> |
||
+ | | |
||
− | |<br> |
||
|A |
|A |
||
|A |
|A |
||
+ | | |
||
− | |<br> |
||
|A |
|A |
||
|- |
|- |
||
| bgcolor="#D0E7FF" align="center" |UV6-0.8 |
| bgcolor="#D0E7FF" align="center" |UV6-0.8 |
||
− | | bgcolor="EEFFFF" | |
||
− | | bgcolor="EEFFFF" | |
||
− | | bgcolor="EEFFFF" | |
||
− | | bgcolor="EEFFFF" | |
||
− | | bgcolor="EEFFFF" |{{rl|Stepper Recipes|Positive Resist (ASML DUV)}} |
||
| |
| |
||
− | | |
+ | | |
+ | | |
||
+ | | |
||
+ | |{{rl|Stepper Recipes|Positive Resist (ASML DUV)}} |
||
+ | | |
||
+ | |- bgcolor="EEFFFF" |
||
| bgcolor="#D0E7FF" align="center" |UV210-0.3 |
| bgcolor="#D0E7FF" align="center" |UV210-0.3 |
||
| |
| |
||
Line 176: | Line 176: | ||
|- |
|- |
||
| bgcolor="#D0E7FF" align="center" |UV26-2.5 |
| bgcolor="#D0E7FF" align="center" |UV26-2.5 |
||
− | | bgcolor="EEFFFF" | |
||
− | | bgcolor="EEFFFF" | |
||
− | | bgcolor="EEFFFF" | |
||
− | | bgcolor="EEFFFF" | |
||
− | | bgcolor="EEFFFF" |A |
||
| |
| |
||
− | | |
+ | | |
+ | | |
||
+ | | |
||
+ | |A |
||
+ | | |
||
+ | |- bgcolor="EEFFFF" |
||
! bgcolor="#D0E7FF" align="center" |'''Negative Resists''' |
! bgcolor="#D0E7FF" align="center" |'''Negative Resists''' |
||
{{LithRecipe Table}} |
{{LithRecipe Table}} |
||
+ | |- |
||
− | |- bgcolor="EEFFFF" |
||
| bgcolor="#D0E7FF" align="center" |AZ5214-EIR |
| bgcolor="#D0E7FF" align="center" |AZ5214-EIR |
||
|{{rl|Contact_Alignment_Recipes|Negative Resist (MJB-3)}} |
|{{rl|Contact_Alignment_Recipes|Negative Resist (MJB-3)}} |
||
Line 193: | Line 193: | ||
| |
| |
||
| |
| |
||
+ | |- bgcolor="EEFFFF" |
||
− | |- |
||
| bgcolor="#D0E7FF" align="center" |AZnLOF 2020 |
| bgcolor="#D0E7FF" align="center" |AZnLOF 2020 |
||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
||
Line 199: | Line 199: | ||
|{{rl|Stepper Recipes|Negative Resist (GCA 6300)}} |
|{{rl|Stepper Recipes|Negative Resist (GCA 6300)}} |
||
|{{rl|Stepper Recipes|Negative Resist (AutoStep 200)}} |
|{{rl|Stepper Recipes|Negative Resist (AutoStep 200)}} |
||
− | | |
||
− | | |
||
− | |- bgcolor="EEFFFF" |
||
− | | bgcolor="#D0E7FF" align="center" |AZnLOF 2035 |
||
− | |A |
||
− | |A |
||
− | |A |
||
− | |A |
||
| |
| |
||
| |
| |
||
|- |
|- |
||
+ | | bgcolor="#D0E7FF" align="center" |AZnLOF 2035 |
||
+ | | bgcolor="EEFFFF" |A |
||
+ | | bgcolor="EEFFFF" |A |
||
+ | | bgcolor="EEFFFF" |A |
||
+ | | bgcolor="EEFFFF" |A |
||
+ | | bgcolor="EEFFFF" | |
||
+ | | bgcolor="EEFFFF" | |
||
+ | |- bgcolor="EEFFFF" |
||
| bgcolor="#D0E7FF" align="center" |AZnLOF 2070 |
| bgcolor="#D0E7FF" align="center" |AZnLOF 2070 |
||
|A |
|A |
||
Line 217: | Line 217: | ||
| |
| |
||
| |
| |
||
+ | |- |
||
− | |- bgcolor="EEFFFF" |
||
| bgcolor="#D0E7FF" align="center" |AZnLOF 5510 |
| bgcolor="#D0E7FF" align="center" |AZnLOF 5510 |
||
|A |
|A |
||
Line 225: | Line 225: | ||
| |
| |
||
| |
| |
||
+ | |- bgcolor="EEFFFF" |
||
− | |- |
||
| bgcolor="#D0E7FF" align="center" |UVN30-0.8 |
| bgcolor="#D0E7FF" align="center" |UVN30-0.8 |
||
| |
| |
||
Line 233: | Line 233: | ||
|{{rl|Stepper Recipes|Negative Resist (ASML DUV)}} |
|{{rl|Stepper Recipes|Negative Resist (ASML DUV)}} |
||
| |
| |
||
+ | |- |
||
− | |- bgcolor="EEFFFF" |
||
| bgcolor="#D0E7FF" align="center" |SU-8 2005,2010, 2015 |
| bgcolor="#D0E7FF" align="center" |SU-8 2005,2010, 2015 |
||
− | |A |
+ | | A |
− | |{{rl|Contact_Alignment_Recipes|Negative Resist (MA-6)}} |
+ | | {{rl|Contact_Alignment_Recipes|Negative Resist (MA-6)}} |
− | |A |
+ | | A |
− | |A |
+ | | A |
| |
| |
||
| |
| |
||
+ | |- bgcolor="EEFFFF" |
||
− | |- |
||
| bgcolor="#D0E7FF" align="center" |SU-8 2075 |
| bgcolor="#D0E7FF" align="center" |SU-8 2075 |
||
|A |
|A |
||
Line 249: | Line 249: | ||
| |
| |
||
| |
| |
||
+ | |- |
||
− | |- bgcolor="EEFFFF" |
||
| bgcolor="#D0E7FF" align="center" |NR9-1000,3000,6000PY |
| bgcolor="#D0E7FF" align="center" |NR9-1000,3000,6000PY |
||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
||
Line 257: | Line 257: | ||
| |
| |
||
| |
| |
||
+ | |- bgcolor="EEFFFF" |
||
− | |- |
||
! bgcolor="#D0E7FF" align="center" | '''Anti-Reflection Coatings''' |
! bgcolor="#D0E7FF" align="center" | '''Anti-Reflection Coatings''' |
||
{{LithRecipe Table}} |
{{LithRecipe Table}} |
||
+ | |- |
||
− | |- bgcolor="EEFFFF" |
||
| bgcolor="#D0E7FF" align="center" |DUV42-P |
| bgcolor="#D0E7FF" align="center" |DUV42-P |
||
| |
| |
||
Line 268: | Line 268: | ||
|{{rl|Stepper Recipes|DUV-42P}} |
|{{rl|Stepper Recipes|DUV-42P}} |
||
| |
| |
||
+ | |- bgcolor="EEFFFF" |
||
− | |- |
||
| bgcolor="#D0E7FF" align="center" |DS-K101-304 |
| bgcolor="#D0E7FF" align="center" |DS-K101-304 |
||
| |
| |
Revision as of 23:04, 13 September 2020
General Information
This page contains information and links to recipes/datasheets spin-coated materials used in the facility.
Table of Contents |
---|
|
Photolithography Recipes
- R = Recipe is available. Clicking this link will take you to the recipe.
- A = Material is available for use, but no recipes are provided.
Photolithography Recipes
| ||||||
---|---|---|---|---|---|---|
Contact Aligner Recipes | Stepper Recipes | Other | ||||
Positive Resists | SUSS MJB-3 | SUSS MA-6 | Stepper 1 (GCA 6300) |
Stepper 2 (AutoStep 200) |
Stepper 3 (ASML DUV) |
MLA150 (Heidelberg) |
AZ4110 | R | R | A | A | ||
AZ4210 | R | R | A | A | ||
AZ4330RS | R | R | A | A | ||
AZ4620 | A | |||||
OCG 825-35CS | A | A | A | A | ||
SPR 950-0.8 | A | A | A | A | ||
SPR 955 CM-0.9 | A | R | R | R | ||
SPR 955 CM-1.8 | A | A | R | R | ||
SPR 220-3.0 | R | R | R | R | ||
SPR 220-7.0 | R | R | R | R | ||
THMR-IP3600 HP D | A | A | A | |||
UV6-0.8 | R | |||||
UV210-0.3 | R | |||||
UV26-2.5 | A | |||||
Negative Resists | SUSS MJB-3 | SUSS MA-6 | Stepper 1 (GCA 6300) |
Stepper 2 (AutoStep 200) |
Stepper 3 (ASML DUV) |
MLA150 (Heidelberg) |
AZ5214-EIR | R | R | R | R | ||
AZnLOF 2020 | R | R | R | R | ||
AZnLOF 2035 | A | A | A | A | ||
AZnLOF 2070 | A | A | A | A | ||
AZnLOF 5510 | A | A | R | R | ||
UVN30-0.8 | R | |||||
SU-8 2005,2010, 2015 | A | R | A | A | ||
SU-8 2075 | A | A | A | A | ||
NR9-1000,3000,6000PY | R | R | A | R | ||
Anti-Reflection Coatings | SUSS MJB-3 | SUSS MA-6 | Stepper 1 (GCA 6300) |
Stepper 2 (AutoStep 200) |
Stepper 3 (ASML DUV) |
MLA150 (Heidelberg) |
DUV42-P | R | |||||
DS-K101-304 | R | |||||
SUSS MJB-3 | SUSS MA-6 | Stepper 1 (GCA 6300) |
Stepper 2 (AutoStep 200) |
Stepper 3 (ASML DUV) |
MLA150 (Heidelberg) |
E-Beam Lithography Recipes (JEOL JBX-6300FS)
- Under Development.
FIB Lithography Recipes (Raith Velion)
To Be Added
Automated Coat/Develop System Recipes (S-Cubed Flexi)
Recipes pre-loaded on the S-Cubed Flexi automated coat/bake/develop system. Only staff may write new recipes, contact the tool supervisor for more info.
To Be Added
Nanoimprinting Recipes
- Thermal Nanoimprint Process and Tutorial
- UV-Cure Low Temp, Low Pressure, Soft-Stamp Nanoimprint Process
Holography Recipes
- Standard Holography Process - on SiO2 on Si
- Holography Process Variations - Set-up Angle - Etching into SiO2 and Si
- Etch SiO2 Nano-structure - Changing Side-wall Angle - Etching into Si with a different line-width
- Reduce SiO2 Nanowire Diameter - Thermal Oxidation - Vapor HF Etching
Low-K Spin-On Dielectric Recipes
Lift-Off Techniques
- Lift-Off Description/Tutorial
- How it works, process limits and considerations for designing your process
- I-Line Lift-Off: Bi-Layer Process with PMGI Underlayer and Contact Aligner
- DUV Lift-Off: UV6 Imaging Resist + PMGI Underlayer
Chemicals Stocked + Datasheets
The following is a list of the lithography chemicals we stock in the lab, with links to the datasheets for each. The datasheets will often have important processing info such as spin-speed vs. thickness curves, typical process parameters, bake temps/times etc.