Difference between revisions of "Lift-Off with DUV Imaging + PMGI Underlayer"
(separated Process Limits into separate section) |
(annotated image caption) |
||
Line 40: | Line 40: | ||
Optionally can use lift-pins & Recipe "'''00 220deg, 3min Vac'''"; |
Optionally can use lift-pins & Recipe "'''00 220deg, 3min Vac'''"; |
||
− | --> Enable Vacuum with overhead valve, only for wafer landing and then turn off |
+ | --> TO prevent wafer sliding: Enable Vacuum with overhead valve, only for wafer landing and then turn off. |
|- |
|- |
||
|Spin UV-6-0.8 @ rcp 6 (3.5krpm) |
|Spin UV-6-0.8 @ rcp 6 (3.5krpm) |
||
Line 85: | Line 85: | ||
===Images / Examples=== |
===Images / Examples=== |
||
− | [[File:PMGI+UV6 lift-off SEM - 2017-06-30 DJ.png|alt=SEM of PR cross-section|none|thumb|578x578px|SEM of holes in PR with above process. Lateral measurement of undercut is only approximate because circle may not have been cut through the exact diameter. (Demis D. John, 2017)]] |
+ | [[File:PMGI+UV6 lift-off SEM - 2017-06-30 DJ.png|alt=SEM of PR cross-section|none|thumb|578x578px|SEM of holes in PR with above process. Top layer is UV6, 140nm underlayer is PMGI, substrate is Silicon. Lateral measurement of undercut is only approximate because circle may not have been cut through the exact diameter. (Demis D. John, 2017)]] |
<br /> |
<br /> |
Revision as of 18:03, 24 June 2020
Developed by Demis D. John, ~2017-2019
This process is intended for Deep-UV Exposure on the ASML DUV Stepper. PMGI is used as the underlayer, which is exposed at the same time as the imaging resist.
Adjust spin speed or switch to a different PMGI formulation to tailor the underlayer thickness to your desired metal thickness.
Tips
Please see our [Bi-Layer Lift-Off Tutorial] to understand the limitations and requirements for good lift-off.
- Remember that gaps in between adjacent metal traces can lift-off during the develop!
- Need underlayer thickness 2x to 3x the desired metal thickness.
- The underlayer will develop laterally from both sides which can lift-off the imaging resist, so:
- Minimum gap between adjacent metals should then be: less than 0.5 * underlayer thickness
- Want at least 30-50nm of underlayer width left to support the imaging resist, so the PR doesn't fall over/collapse.
- Make sure to use a vertical evaporation - EBeam4 or EBeam1. EBeam3 is not vertical.
Process Limits
This process is written with PMGI SF-5 @ 4krpm, which spins to about 130nm
- Maximum metal thickness = 130nm/3 ≈ 45nm
- Undercuts laterally about 130-140nm, so minimum gap between metals = (2 x 140nm) + ~30nm ≈ 350nm
Adjust the PMGI layer thickness to adjust these process limits.
Suggested Process for Liftoff
De-H2O Bake (eg. 220°C, 1m+)
- or - Technics O2 ash (300mT, 100W), 15sec |
Oxygen ash is faster and more effective |
Spin PMGI SF-5 @ 4krpm (rcp 7) | |
POLOS underside clean: 2000rpm, ACE/ISO/N2 | |
PMGI-Bake: 220°C, 3min (BrewerSci lift-pin hotplate). | Can just place wafer directly onto hotplate surface.
Optionally can use lift-pins & Recipe "00 220deg, 3min Vac"; --> TO prevent wafer sliding: Enable Vacuum with overhead valve, only for wafer landing and then turn off. |
Spin UV-6-0.8 @ rcp 6 (3.5krpm) | |
POLOS underside clean: 2000rpm, ACE/ISO/N2 | |
Soft-Bake = 135°C, 1min (builtin hotplate) | |
(check underside for particulates) | |
ASML Exposure | |
Default: Exp = 37.5mJ // foc = –0.10 | Try this exposure dose but might need to do a FocArray (smaller Image Distribution eg. 5x5) to find proper exposure. |
PEB = 135°C, 1.5min (built-in hotplate) | |
Dev (300MiF) = 50sec (CRITICAL time) | Use cassette & H2O rinse dish prepared
--> not stirring, instead very slow/gentle lift/drop at various angles or gentle swish just to mix developer slightly. |
DI rinse | Very Gently! Dunk into prepared DI dish, and dump/fill gently 2x. Don’t allow direct hard water to hit PR surface. |
PEii Technics O2: 30sec (100W/300mT) | May increase feature size openings by ~50nm. |
Metal Evaporation
(insert steps) |
EBeam#4 or EBeam#1 with vertical/4-inch holders (not planetary) |
Lift-off in NMP | Facing down or vertical. |
Data
• For PMGI Baked at 220°C for 3min, the PMGI dissolves in AZ 300MIF at a rate of approximately ~600nm/min.
Images / Examples