Difference between revisions of "InP Etch Rate and Selectivity (InP/SiO2)"
Jump to navigation
Jump to search
Line 1: | Line 1: | ||
{| class="wikitable" |
{| class="wikitable" |
||
− | | colspan="3" |1.4 mT, 125/800W, Cl2/H2/Ar flow-rate=6.3/12.7/2 sccm, chuck temperature=200 C, and etch time=90s (Prior to the etch, do O2 plasma chamber clean for 15 minutes, then, chamber coating with the same recipe and a quarter dummy InP on carrier |
+ | | colspan="3" |1.4 mT, 125/800W, Cl2/H2/Ar flow-rate=6.3/12.7/2 sccm, chuck temperature=200 C, and etch time=90s (Prior to the etch, do O2 plasma chamber clean for 15 minutes, then, chamber coating with the same recipe and a quarter dummy InP on carrier for 15 minutes. |
|- |
|- |
||
|Date |
|Date |
Revision as of 16:08, 27 April 2018
1.4 mT, 125/800W, Cl2/H2/Ar flow-rate=6.3/12.7/2 sccm, chuck temperature=200 C, and etch time=90s (Prior to the etch, do O2 plasma chamber clean for 15 minutes, then, chamber coating with the same recipe and a quarter dummy InP on carrier for 15 minutes. | ||
Date | InP Etch Rtae (mm/min) | Selectivity (InP/SiO2) |
4/10/2018 | 1.12 | 12.8 |
6/26/2018 | 1.29 | 13.6 |