Difference between revisions of "Dry Etching Recipes"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
(lkink change)
(link to Oxford InP/PnGaAsP recipes)
 
(18 intermediate revisions by 4 users not shown)
Line 1: Line 1:
 
{{Recipe Table Explanation}}
 
{{Recipe Table Explanation}}
 +
 
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
 
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
 
|- bgcolor="#d0e7ff"
 
|- bgcolor="#d0e7ff"
Line 5: Line 6:
 
|- bgcolor="#d0e7ff"
 
|- bgcolor="#d0e7ff"
 
|<!-- INTENTIONALLY LEFT BLANK -->
 
|<!-- INTENTIONALLY LEFT BLANK -->
! colspan="4" width="300" height="35" align="center" bgcolor="#d0e7ff" |'''[[RIE Etching Recipes|RIE Etching]]'''
+
! colspan="3" |'''[[RIE Etching Recipes|RIE Etching]]'''
! colspan="5" |'''[[ICP Etching Recipes|ICP Etching]]'''
+
! colspan="6" |'''[[ICP Etching Recipes|ICP Etching]]'''
! colspan="5" align="center" bgcolor="#d0e7ff" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
+
! colspan="5" bgcolor="#d0e7ff" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
! colspan="3" align="center" bgcolor="#d0e7ff" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
+
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
 
|-
 
|-
! width="65" align="center" bgcolor="#d0e7ff" |'''Material'''
+
! bgcolor="#d0e7ff" align="center" |'''Material'''
| width="65" bgcolor="#daf1ff" |[[RIE 1 (Custom)|RIE 1<br>(Retired)]]
+
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]]
| width="65" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
+
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> <span style="font-size: 88%;">(MRC)</span>]]
| width="65" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
+
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| width="100" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]]
+
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| width="100" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]]
+
| bgcolor="#daf1ff" |[[Fluorine ICP Etcher (PlasmaTherm/SLR Fluorine ICP)|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]]
| width="100" bgcolor="#daf1ff" |[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#PlasmaTherm.2FSLR_Fluorine_Etcher SLR Fluorine ICP (PlasmaTherm)]
+
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]]
| width="120" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic 1)]]
+
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]]
| width="120" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic 2)]]
+
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]]
| width="85" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br>(Unaxis VLR)]]
+
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br><span style="font-size: 88%;">(Unaxis VLR)</span>]]
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
+
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]]
| width="95" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
+
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br><span style="font-size: 88%;">(Gasonics 2000)</span>]]
| width="95" bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean (YES EcoClean)]]
+
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]]
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
+
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
+
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br><span style="font-size: 88%;">(EVG 810)</span>]]
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]]
+
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br><span style="font-size: 88%;">(Xetch)</span>]]
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]]
+
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br><span style="font-size: 88%;">(uETCH)</span>]]
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
+
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br><span style="font-size: 88%;">(Oxford)</span>]]
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Ag
+
! bgcolor="#d0e7ff" align="center" |Ag
 
|
 
|
 
|
 
|
Line 46: Line 47:
 
|
 
|
 
|
 
|
|
+
|A
|- bgcolor="#eeffff"
+
|- bgcolor="#ffffff"
! align="center" bgcolor="#d0e7ff" |Al
+
! bgcolor="#d0e7ff" align="center" |Al
|
 
 
|
 
|
 
|
 
|
Line 66: Line 66:
 
|
 
|
 
|
 
|
 +
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Au
+
! bgcolor="#d0e7ff" align="center" |Au
 
|
 
|
 
|
 
|
Line 84: Line 85:
 
|
 
|
 
|
 
|
|[https://www.nanotech.ucsb.edu/wiki/index.php/Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29 A]
+
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|- bgcolor="#eeffff"
+
|- bgcolor="#ffffff"
! align="center" bgcolor="#d0e7ff" |Cr
+
! bgcolor="#d0e7ff" align="center" |Cr
|
 
 
|
 
|
 
|
 
|
Line 104: Line 104:
 
|
 
|
 
|
 
|
 +
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Cu
+
! bgcolor="#d0e7ff" align="center" |Cu
 
|
 
|
 
|
 
|
Line 122: Line 123:
 
|
 
|
 
|
 
|
 +
|A
 +
|- bgcolor="#ffffff"
 +
! bgcolor="#d0e7ff" align="center" |Ge
 
|
 
|
|-
 
! align="center" bgcolor="#d0e7ff" |Ge
 
 
|
 
|
 
|
 
|
Line 138: Line 140:
 
|
 
|
 
|
 
|
 +
|A
 
|
 
|
 
|A
 
|A
|
 
|
 
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Mo
+
! bgcolor="#d0e7ff" align="center" |Mo
 
|
 
|
 
|
 
|
Line 160: Line 161:
 
|
 
|
 
|
 
|
|
+
|A
|-
+
|- bgcolor="#ffffff"
! align="center" bgcolor="#d0e7ff" |Ni
+
! bgcolor="#d0e7ff" align="center" |Ni
 
|
 
|
 
|
 
|
Line 180: Line 181:
 
|
 
|
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
+
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Pt
+
! bgcolor="#d0e7ff" align="center" |Pt
 
|
 
|
 
|
 
|
Line 199: Line 200:
 
|
 
|
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
+
|- bgcolor="#ffffff"
! align="center" bgcolor="#d0e7ff" |Ru
+
! bgcolor="#d0e7ff" align="center" |Ru
|
 
 
|
 
|
 
|
 
|
Line 218: Line 218:
 
|
 
|
 
|
 
|
 +
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Si
+
! bgcolor="#d0e7ff" align="center" |Si
|
 
 
|
 
|
 
|
 
|
Line 228: Line 228:
 
|
 
|
 
|
 
|
 +
|A
 
|
 
|
 
|
 
|
Line 236: Line 237:
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (XeF2 Etcher)}}
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (XeF2 Etcher)}}
 
|
 
|
 +
|A
 +
|- bgcolor="#ffffff"
 +
! bgcolor="#d0e7ff" align="center" |Ta
 
|
 
|
|-
 
! align="center" bgcolor="#d0e7ff" |Ta
 
 
|
 
|
 
|
 
|
Line 254: Line 256:
 
|
 
|
 
|
 
|
|
+
|A
|
+
|- bgcolor="#eeffff"
|-
+
! bgcolor="#d0e7ff" align="center" |Ti
! align="center" bgcolor="#d0e7ff" |Ti
 
|
 
 
|
 
|
 
|
 
|
Line 275: Line 275:
 
|
 
|
 
|
 
|
|-
+
|A
! align="center" bgcolor="#d0e7ff" |Al<sub>2</sub>O<sub>3</sub>
+
|- bgcolor="#ffffff"
 +
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub>
 
|
 
|
 
|
 
|
Line 283: Line 284:
 
|
 
|
 
|
 
|
|
+
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R]
|[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R]
 
 
|
 
|
 
|
 
|
Line 294: Line 294:
 
|
 
|
 
|
 
|
 +
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub>
+
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub>
|
 
 
|
 
|
 
|
 
|
Line 313: Line 313:
 
|
 
|
 
|
 
|
|-
+
|A
! align="center" bgcolor="#d0e7ff" |AlGaAs
+
|- bgcolor="#ffffff"
|
+
! bgcolor="#d0e7ff" align="center" |AlGaAs
 
|
 
|
 
|
 
|
Line 323: Line 323:
 
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}}
 
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}}
 
|
 
|
 +
|A
 
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}}
 
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}}
 
|
 
|
Line 331: Line 332:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |AlGaN
+
! bgcolor="#d0e7ff" align="center" |AlGaN
|
 
 
|
 
|
 
|
 
|
Line 342: Line 342:
 
|
 
|
 
|
 
|
 +
|A
 
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
 
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
 
|
 
|
Line 350: Line 351:
 
|
 
|
 
|
 
|
|
+
|A
|-
+
|- bgcolor="#ffffff"
! align="center" bgcolor="#d0e7ff" |AlN
+
! bgcolor="#d0e7ff" align="center" |AlN
 
|
 
|
 
|
 
|
Line 369: Line 370:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |CdZnTe
+
! bgcolor="#d0e7ff" align="center" |CdZnTe
|
 
 
|{{rl|RIE Etching Recipes|CdZnTe Etch (RIE 2)}}
 
|{{rl|RIE Etching Recipes|CdZnTe Etch (RIE 2)}}
 
|
 
|
Line 389: Line 389:
 
|
 
|
 
|
 
|
|- bgcolor="#eeffff"
+
|A
! align="center" bgcolor="#d0e7ff" |GaAs
+
|- bgcolor="#ffffff"
|
+
! bgcolor="#d0e7ff" align="center" |GaAs
 
|
 
|
 
|
 
|
Line 399: Line 399:
 
|{{rl|ICP Etching Recipes|GaAs-AlGaAs_Etch_.28Panasonic_1.29}}
 
|{{rl|ICP Etching Recipes|GaAs-AlGaAs_Etch_.28Panasonic_1.29}}
 
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}}
 
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}}
 +
|A
 
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}}
 
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}}
 
|
 
|
Line 407: Line 408:
 
|
 
|
 
|
 
|
|
+
|A
|-
+
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |GaN
+
! bgcolor="#d0e7ff" align="center" |GaN
|
 
 
|
 
|
 
|
 
|
Line 418: Line 418:
 
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}}
 
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}}
 
|
 
|
 +
|A
 
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
 
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}}
 
|
 
|
Line 426: Line 427:
 
|
 
|
 
|
 
|
|
+
|A
|- bgcolor="#eeffff"
+
|- bgcolor="#ffffff"
! align="center" bgcolor="#d0e7ff" |GaSb
+
! bgcolor="#d0e7ff" align="center" |GaSb
 
|
 
|
 
|
 
|
Line 435: Line 436:
 
|
 
|
 
|
 
|
 +
|A
 
|
 
|
|A
 
 
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}}
 
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}}
 
|
 
|
Line 445: Line 446:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |HfO<sub>2</sub>
+
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub>
 
|
 
|
 
|
 
|
Line 464: Line 465:
 
|
 
|
 
|
 
|
|
+
|A
|- bgcolor="#eeffff"
+
|- bgcolor="#ffffff"
! align="center" bgcolor="#d0e7ff" |InGaAlAs
+
! bgcolor="#d0e7ff" align="center" |InGaAlAs
|
 
 
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
 
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
 
|
 
|
Line 475: Line 475:
 
|
 
|
 
|
 
|
 +
|A
 
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
 
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
 
|
 
|
Line 483: Line 484:
 
|
 
|
 
|
 
|
|
+
|A
|-
+
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |InGaAsP
+
! bgcolor="#d0e7ff" align="center" |InGaAsP
|
 
 
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
 
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
 
|
 
|
Line 494: Line 494:
 
|
 
|
 
|
 
|
 +
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R]]
 
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
 
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
 
|
 
|
Line 502: Line 503:
 
|
 
|
 
|
 
|
|
+
|A
|- bgcolor="#eeffff"
+
|- bgcolor="#ffffff"
! align="center" bgcolor="#d0e7ff" |InP
+
! bgcolor="#d0e7ff" align="center" |InP
|
 
 
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
 
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
 
|
 
|
Line 513: Line 513:
 
|A
 
|A
 
|A
 
|A
 +
|[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R]]
 
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
 
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}}
 
|
 
|
Line 521: Line 522:
 
|
 
|
 
|
 
|
|
+
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|-
+
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |ITO
+
! bgcolor="#d0e7ff" align="center" |ITO
|
 
 
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}}
 
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}}
 
|
 
|
Line 541: Line 541:
 
|
 
|
 
|
 
|
|- bgcolor="#eeffff"
+
|A
 +
|- bgcolor="#ffffff"
 
!Photoresist
 
!Photoresist
 
& ARC
 
& ARC
|
 
 
|
 
|
 
|A
 
|A
|[https://www.nanotech.ucsb.edu/wiki/index.php/RIE_Etching_Recipes#Photoresist_and_ARC R]
+
|[https://wiki.nanotech.ucsb.edu/wiki/RIE_Etching_Recipes#Photoresist_and_ARC_.28RIE_5.29 R]
 
|
 
|
 +
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_.26_ARC_.28Fluorine_ICP_Etcher.29 R]
 +
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 R]
 +
|[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_etching_.28Panasonic_2.29 R]
 
|
 
|
|[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_Etching R]
 
|[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_etching_2 R]
 
 
|
 
|
 +
|A
 
|A
 
|A
 
|A
 
|A
Line 559: Line 561:
 
|
 
|
 
|
 
|
|
+
|A
|
+
|- bgcolor="#eeffff"
|-
+
! bgcolor="#d0e7ff" align="center" |SiC
! align="center" bgcolor="#d0e7ff" |SiC
 
|
 
 
|
 
|
 
|
 
|
Line 580: Line 580:
 
|
 
|
 
|
 
|
|-
+
|A
! align="center" bgcolor="#d0e7ff" |SiN
+
|- bgcolor="#ffffff"
|
+
! bgcolor="#d0e7ff" align="center" |SiN
 
|
 
|
 
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}}
 
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}}
 
|
 
|
 
|
 
|
|
+
|A
 
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}}
 
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}}
 
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 2)}}
 
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 2)}}
 +
|
 
|
 
|
 
|A
 
|A
Line 598: Line 599:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |SiO<sub>2</sub>
+
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub>
|
 
 
|
 
|
 
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}}
 
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}}
 
|
 
|
 
|
 
|
|A
+
|{{rl|ICP Etching Recipes|SiO2 Etching (Fluorine ICP Etcher)}}
 
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}}
 
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}}
 
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 2)}}
 
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 2)}}
 +
|
 
|
 
|
 
|
 
|
Line 617: Line 618:
 
|
 
|
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}}
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}}
|
+
|A
|- bgcolor="#eeffff"
+
|- bgcolor="#ffffff"
! align="center" bgcolor="#d0e7ff" |SiOxNy
+
! bgcolor="#d0e7ff" align="center" |SiOxNy
|
 
 
|
 
|
 
|
 
|
Line 637: Line 637:
 
|
 
|
 
|
 
|
|-
+
|A
! align="center" bgcolor="#d0e7ff" |Ta<sub>2</sub>O<sub>5</sub>
+
|- bgcolor="#eeffff"
|
+
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub>
 
|
 
|
 
|
 
|
Line 656: Line 656:
 
|
 
|
 
|
 
|
|-
+
|A
! align="center" bgcolor="#d0e7ff" |TiN
+
|- bgcolor="#ffffff"
|
+
! bgcolor="#d0e7ff" align="center" |TiN
 
|
 
|
 
|
 
|
Line 675: Line 675:
 
|
 
|
 
|
 
|
 +
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |TiO<sub>2</sub>
+
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub>
 
|
 
|
 
|
 
|
Line 693: Line 694:
 
|
 
|
 
|
 
|
|
+
|A
|- bgcolor="#eeffff"
+
|- bgcolor="#ffffff"
! align="center" bgcolor="#d0e7ff" |W-TiW
+
! bgcolor="#d0e7ff" align="center" |W-TiW
|
 
 
|
 
|
 
|
 
|
Line 713: Line 713:
 
|
 
|
 
|
 
|
 +
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |ZnO<sub>2</sub>
+
! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub>
 
|
 
|
 
|
 
|
Line 731: Line 732:
 
|
 
|
 
|
 
|
|
+
|A
|-
+
|- bgcolor="#ffffff"
! align="center" bgcolor="#d0e7ff" |ZnS
+
! bgcolor="#d0e7ff" align="center" |ZnS
|
 
 
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
 
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
 
|
 
|
Line 751: Line 751:
 
|
 
|
 
|
 
|
|-
+
|A
! align="center" bgcolor="#d0e7ff" |ZnSe
+
|- bgcolor="#eeffff"
|
+
! bgcolor="#d0e7ff" align="center" |ZnSe
 
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
 
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
 
|
 
|
Line 770: Line 770:
 
|
 
|
 
|
 
|
|-
+
|A
! align="center" bgcolor="#d0e7ff" |ZrO<sub>2</sub>
+
|- bgcolor="#ffffff"
 +
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub>
 
|
 
|
 
|
 
|
Line 788: Line 789:
 
|
 
|
 
|
 
|
|
+
|A
|-
+
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |'''Material'''
+
! bgcolor="#d0e7ff" align="center" |'''Material'''
| bgcolor="#daf1ff" |[[RIE 1 (Custom)|RIE 1<br>(Retired)]]
+
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
+
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> <span style="font-size: 88%;">(MRC)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
+
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]]
+
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]]
+
| bgcolor="#daf1ff" |[[Fluorine ICP Etcher (PlasmaTherm/SLR Fluorine ICP)|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]]
| bgcolor="#daf1ff" |[[Fluorine ICP Etcher (PlasmaTherm/SLR Fluorine ICP)|SLR Fluorine ICP (PlasmaTherm)]]
+
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic E626I)]]
+
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic E640)]]
+
| bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]]
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br>(Unaxis VLR)]]
+
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br><span style="font-size: 88%;">(Unaxis VLR)</span>]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
+
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
+
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br><span style="font-size: 88%;">(Gasonics 2000)</span>]]
| bgcolor="#daf1ff" |[[Plasma Clean (YES EcoClean)]]
+
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]]
 
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
 
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
+
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br><span style="font-size: 88%;">(EVG 810)</span>]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]]
+
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br><span style="font-size: 88%;">(Xetch)</span>]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]]
+
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br><span style="font-size: 88%;">(uETCH)</span>]]
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
+
| bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br><span style="font-size: 88%;">(Oxford)</span>]]
 
|}
 
|}
  
 
[[Category:Processing]]
 
[[Category:Processing]]

Latest revision as of 13:53, 8 October 2021

  • R = Recipe is available. Clicking this link will take you to the recipe.
  • A = Material is available for use, but no recipes are provided.
Dry Etching Recipes
RIE Etching ICP Etching Oxygen Plasma Systems Other Dry Etchers
Material RIE 2
(MRC)
RIE 3
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic E626I)
ICP Etch 2
(Panasonic E640)
Oxford ICP (PlasmaPro 100) ICP-Etch
(Unaxis VLR)
Ashers
(Technics PEII)
Plasma Clean
(Gasonics 2000)
Plasma Clean (YES EcoClean) UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)
Ag A
Al A R R A
Au R
Cr A R A A
Cu A
Ge A A
Mo A
Ni R
Pt R
Ru A R A
Si R R A R A
Ta A
Ti R A A
Al2O3 R A
Al2O3 (Sapphire) R A A
AlGaAs R R A R A
AlGaN A R A
AlN R A
CdZnTe R A
GaAs R R R A R A
GaN R R A R A
GaSb A R A
HfO2 A
InGaAlAs R A R A
InGaAsP R R R A
InP R A A R R R
ITO R A
Photoresist

& ARC

A R R R R A A A A
SiC R A A
SiN R A R R A A
SiO2 R R R R R A
SiOxNy A A A
Ta2O5 A A
TiN A
TiO2 A
W-TiW R A A
ZnO2 A
ZnS R A
ZnSe R A
ZrO2 A
Material RIE 2
(MRC)
RIE 3
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic E626I)
ICP Etch 2
(Panasonic E640)
Oxford ICP (PlasmaPro 100) ICP-Etch
(Unaxis VLR)
Ashers
(Technics PEII)
Plasma Clean
(Gasonics 2000)
Plasma Clean (YES EcoClean) UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)