Difference between revisions of "Dry Etching Recipes"
Jump to navigation
Jump to search
(Updated formatting- smaller font for model #, header colors) |
m (fix incorrect color header cell) |
||
(14 intermediate revisions by 3 users not shown) | |||
Line 1: | Line 1: | ||
+ | ===<u>[[Process Group - Process Control Data#Etching .28Process Control Data.29|Process Control Data]]</u>=== |
||
− | {{Recipe Table Explanation}} |
||
+ | <small>''See [[Process Group - Process Control Data#Etching .28Process Control Data.29|linked page]] for [https://en.wikipedia.org/wiki/Statistical_process_control process control data] (dep rate/stress etc. over time), for a selection of often-used thin-film depositions.''</small> |
||
+ | |||
+ | ===Dry Etching Tools/Materials Table=== |
||
+ | |||
+ | *<small>'''R''': ''Recipe is available. Clicking this link will take you to the recipe.''</small> |
||
+ | *<small>'''A''': ''Material is available for use, but no recipes are provided.''</small> |
||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1" |
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1" |
||
+ | |- |
||
− | |- bgcolor="#d0e7ff" |
||
! colspan="18" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div> |
! colspan="18" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div> |
||
|- bgcolor="#d0e7ff" |
|- bgcolor="#d0e7ff" |
||
− | |<!-- INTENTIONALLY LEFT BLANK --> |
+ | | bgcolor="#eaecf0" | <!-- INTENTIONALLY LEFT BLANK --> |
! colspan="3" |'''[[RIE Etching Recipes|RIE Etching]]''' |
! colspan="3" |'''[[RIE Etching Recipes|RIE Etching]]''' |
||
! colspan="6" |'''[[ICP Etching Recipes|ICP Etching]]''' |
! colspan="6" |'''[[ICP Etching Recipes|ICP Etching]]''' |
||
! colspan="5" bgcolor="#d0e7ff" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]''' |
! colspan="5" bgcolor="#d0e7ff" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]''' |
||
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]''' |
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]''' |
||
+ | |- bgcolor="#d0e7ff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |'''Material''' |
! bgcolor="#d0e7ff" align="center" |'''Material''' |
||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]] |
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]] |
||
Line 16: | Line 22: | ||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
− | | bgcolor="#daf1ff" |[[ |
+ | | bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]] |
||
− | | bgcolor="#daf1ff" |[[Oxford ICP Etcher |
+ | | bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br><span style="font-size: 88%;">(Unaxis VLR)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br><span style="font-size: 88%;">(Unaxis VLR)</span>]] |
||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]] |
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]] |
||
+ | | bgcolor="#daf1ff" | |
||
− | | bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br><span style="font-size: 88%;">(Gasonics 2000)</span>]] |
||
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]] |
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]] |
||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
||
Line 48: | Line 54: | ||
| |
| |
||
|A |
|A |
||
− | |- bgcolor="# |
+ | |- bgcolor="#ffffff" |
! bgcolor="#d0e7ff" align="center" |Al |
! bgcolor="#d0e7ff" align="center" |Al |
||
| |
| |
||
Line 86: | Line 92: | ||
| |
| |
||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
||
− | |- bgcolor="# |
+ | |- bgcolor="#ffffff" |
! bgcolor="#d0e7ff" align="center" |Cr |
! bgcolor="#d0e7ff" align="center" |Cr |
||
| |
| |
||
Line 124: | Line 130: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#ffffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |Ge |
! bgcolor="#d0e7ff" align="center" |Ge |
||
| |
| |
||
Line 131: | Line 137: | ||
| |
| |
||
| |
| |
||
− | | |
+ | |A |
− | | |
+ | |A |
| |
| |
||
| |
| |
||
Line 163: | Line 169: | ||
|A |
|A |
||
|- |
|- |
||
+ | !Nb |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |A |
||
+ | |A |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |- bgcolor="#ffffff" |
||
! bgcolor="#d0e7ff" align="center" |Ni |
! bgcolor="#d0e7ff" align="center" |Ni |
||
| |
| |
||
Line 182: | Line 207: | ||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
||
|- |
|- |
||
+ | !Os |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |A |
||
+ | |A |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |Pt |
! bgcolor="#d0e7ff" align="center" |Pt |
||
| |
| |
||
Line 200: | Line 244: | ||
| |
| |
||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
||
+ | |- bgcolor="#ffffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |Ru |
! bgcolor="#d0e7ff" align="center" |Ru |
||
| |
| |
||
Line 238: | Line 282: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#ffffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |Ta |
! bgcolor="#d0e7ff" align="center" |Ta |
||
| |
| |
||
Line 245: | Line 289: | ||
| |
| |
||
| |
| |
||
− | | |
+ | |A |
− | | |
+ | |A |
| |
| |
||
| |
| |
||
Line 257: | Line 301: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#eeffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |Ti |
! bgcolor="#d0e7ff" align="center" |Ti |
||
| |
| |
||
Line 276: | Line 320: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#ffffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub> |
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub> |
||
| |
| |
||
Line 283: | Line 327: | ||
| |
| |
||
| |
| |
||
− | | |
+ | |A |
− | |[https://wiki.nanotech.ucsb.edu/ |
+ | |[https://wiki.nanotech.ucsb.edu/w/index.php?title=ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R] |
| |
| |
||
| |
| |
||
Line 314: | Line 358: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#ffffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |AlGaAs |
! bgcolor="#d0e7ff" align="center" |AlGaAs |
||
| |
| |
||
Line 323: | Line 367: | ||
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}} |
||
| |
| |
||
+ | |[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R]] |
||
− | | |
||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}} |
||
| |
| |
||
Line 342: | Line 386: | ||
| |
| |
||
| |
| |
||
+ | |[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R]] |
||
− | | |
||
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
||
| |
| |
||
Line 352: | Line 396: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#ffffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |AlN |
! bgcolor="#d0e7ff" align="center" |AlN |
||
| |
| |
||
Line 371: | Line 415: | ||
| |
| |
||
|A |
|A |
||
+ | |- |
||
+ | !BCB |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |A |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |CdZnTe |
! bgcolor="#d0e7ff" align="center" |CdZnTe |
||
Line 390: | Line 453: | ||
| |
| |
||
|A |
|A |
||
− | |- bgcolor="# |
+ | |- bgcolor="#ffffff" |
! bgcolor="#d0e7ff" align="center" |GaAs |
! bgcolor="#d0e7ff" align="center" |GaAs |
||
| |
| |
||
Line 399: | Line 462: | ||
|{{rl|ICP Etching Recipes|GaAs-AlGaAs_Etch_.28Panasonic_1.29}} |
|{{rl|ICP Etching Recipes|GaAs-AlGaAs_Etch_.28Panasonic_1.29}} |
||
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}} |
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}} |
||
+ | |[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R]] |
||
− | |A |
||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}} |
||
| |
| |
||
Line 409: | Line 472: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#eeffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |GaN |
! bgcolor="#d0e7ff" align="center" |GaN |
||
| |
| |
||
Line 417: | Line 480: | ||
| |
| |
||
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}} |
||
− | | |
||
|A |
|A |
||
+ | |[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R]] |
||
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
||
| |
| |
||
Line 428: | Line 491: | ||
| |
| |
||
|A |
|A |
||
− | |- bgcolor="# |
+ | |- bgcolor="#ffffff" |
! bgcolor="#d0e7ff" align="center" |GaSb |
! bgcolor="#d0e7ff" align="center" |GaSb |
||
− | | |
||
| |
| |
||
| |
| |
||
Line 437: | Line 499: | ||
| |
| |
||
|A |
|A |
||
− | | |
+ | |A |
+ | |A |
||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}} |
||
| |
| |
||
Line 466: | Line 529: | ||
| |
| |
||
|A |
|A |
||
− | |- bgcolor="# |
+ | |- bgcolor="#ffffff" |
! bgcolor="#d0e7ff" align="center" |InGaAlAs |
! bgcolor="#d0e7ff" align="center" |InGaAlAs |
||
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
||
Line 485: | Line 548: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#eeffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |InGaAsP |
! bgcolor="#d0e7ff" align="center" |InGaAsP |
||
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
||
Line 494: | Line 557: | ||
| |
| |
||
| |
| |
||
+ | |[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R]] |
||
− | |R |
||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
||
| |
| |
||
Line 504: | Line 567: | ||
| |
| |
||
|A |
|A |
||
− | |- bgcolor="# |
+ | |- bgcolor="#ffffff" |
! bgcolor="#d0e7ff" align="center" |InP |
! bgcolor="#d0e7ff" align="center" |InP |
||
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
||
Line 513: | Line 576: | ||
|A |
|A |
||
|A |
|A |
||
+ | |[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R]] |
||
− | |R |
||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
||
| |
| |
||
Line 523: | Line 586: | ||
| |
| |
||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
||
+ | |- bgcolor="#eeffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |ITO |
! bgcolor="#d0e7ff" align="center" |ITO |
||
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}} |
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}} |
||
Line 542: | Line 605: | ||
| |
| |
||
|A |
|A |
||
+ | |- |
||
− | |- bgcolor="#eeffff" |
||
+ | !LiNbO3 |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |A |
||
+ | |- bgcolor="#ffffff" |
||
!Photoresist |
!Photoresist |
||
& ARC |
& ARC |
||
Line 554: | Line 636: | ||
| |
| |
||
| |
| |
||
− | | |
+ | |R |
− | | |
+ | | |
− | | |
+ | |R |
| |
| |
||
| |
| |
||
Line 563: | Line 645: | ||
|A |
|A |
||
|- |
|- |
||
+ | !Ru |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |A |
||
+ | |[[ICP Etching Recipes#Ru .28Ruthenium.29 Etch .28Panasonic 2.29|R]] |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |- bgcolor="#eeffff" |
||
! bgcolor="#d0e7ff" align="center" |SiC |
! bgcolor="#d0e7ff" align="center" |SiC |
||
| |
| |
||
Line 581: | Line 682: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#ffffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |SiN |
! bgcolor="#d0e7ff" align="center" |SiN |
||
| |
| |
||
Line 587: | Line 688: | ||
| |
| |
||
| |
| |
||
− | | |
+ | |A |
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}} |
||
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 2)}} |
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 2)}} |
||
Line 619: | Line 720: | ||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}} |
|{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}} |
||
|A |
|A |
||
− | |- bgcolor="# |
+ | |- bgcolor="#ffffff" |
! bgcolor="#d0e7ff" align="center" |SiOxNy |
! bgcolor="#d0e7ff" align="center" |SiOxNy |
||
| |
| |
||
Line 639: | Line 740: | ||
|A |
|A |
||
|- |
|- |
||
+ | !SU8 |
||
− | ! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub> |
||
| |
| |
||
| |
| |
||
Line 645: | Line 746: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
| |
| |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |- bgcolor="#eeffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub> |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |A |
||
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A] |
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A] |
||
| |
| |
||
Line 657: | Line 777: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#ffffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |TiN |
! bgcolor="#d0e7ff" align="center" |TiN |
||
| |
| |
||
Line 695: | Line 815: | ||
| |
| |
||
|A |
|A |
||
− | |- bgcolor="# |
+ | |- bgcolor="#ffffff" |
! bgcolor="#d0e7ff" align="center" |W-TiW |
! bgcolor="#d0e7ff" align="center" |W-TiW |
||
| |
| |
||
Line 733: | Line 853: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#ffffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |ZnS |
! bgcolor="#d0e7ff" align="center" |ZnS |
||
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}} |
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}} |
||
Line 752: | Line 872: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#eeffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |ZnSe |
! bgcolor="#d0e7ff" align="center" |ZnSe |
||
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}} |
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}} |
||
Line 771: | Line 891: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#ffffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub> |
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub> |
||
| |
| |
||
Line 790: | Line 910: | ||
| |
| |
||
|A |
|A |
||
+ | |- bgcolor="#eeffff" |
||
− | |- |
||
! bgcolor="#d0e7ff" align="center" |'''Material''' |
! bgcolor="#d0e7ff" align="center" |'''Material''' |
||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]] |
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]] |
||
Line 796: | Line 916: | ||
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
− | | bgcolor="#daf1ff" |[[ |
+ | | bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]] |
||
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]] |
||
− | | bgcolor="#daf1ff" |[[Oxford ICP Etcher |
+ | | bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br><span style="font-size: 88%;">(Unaxis VLR)</span>]] |
| bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br><span style="font-size: 88%;">(Unaxis VLR)</span>]] |
||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]] |
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]] |
||
+ | | |
||
− | | bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br><span style="font-size: 88%;">(Gasonics 2000)</span>]] |
||
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]] |
| bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]] |
||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
Revision as of 16:54, 29 September 2022
Process Control Data
See linked page for process control data (dep rate/stress etc. over time), for a selection of often-used thin-film depositions.
Dry Etching Tools/Materials Table
- R: Recipe is available. Clicking this link will take you to the recipe.
- A: Material is available for use, but no recipes are provided.