Difference between revisions of "Dry Etching Recipes"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
(10 intermediate revisions by 4 users not shown)
Line 2: Line 2:
 
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
 
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1"
 
|- bgcolor="#d0e7ff"
 
|- bgcolor="#d0e7ff"
! colspan="18" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div>
+
! colspan="17" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div>
 
|- bgcolor="#d0e7ff"
 
|- bgcolor="#d0e7ff"
 
|<!-- INTENTIONALLY LEFT BLANK -->
 
|<!-- INTENTIONALLY LEFT BLANK -->
! colspan="4" width="300" height="35" align="center" bgcolor="#d0e7ff" |'''[[RIE Etching Recipes|RIE Etching]]'''
+
! colspan="3" |'''[[RIE Etching Recipes|RIE Etching]]'''
 
! colspan="5" |'''[[ICP Etching Recipes|ICP Etching]]'''
 
! colspan="5" |'''[[ICP Etching Recipes|ICP Etching]]'''
! colspan="5" align="center" bgcolor="#d0e7ff" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
+
! colspan="5" bgcolor="#d0e7ff" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]'''
! colspan="3" align="center" bgcolor="#d0e7ff" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
+
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]'''
 
|-
 
|-
! width="65" align="center" bgcolor="#d0e7ff" |'''Material'''
+
! width="65" bgcolor="#d0e7ff" align="center" |'''Material'''
| width="65" bgcolor="#daf1ff" |[[RIE 1 (Custom)|RIE 1<br>(Retired)]]
 
 
| width="65" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
 
| width="65" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
 
| width="65" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
 
| width="65" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
 
| width="100" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]]
 
| width="100" bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br>(PlasmaTherm)]]
 
| width="100" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]]
 
| width="100" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]]
| width="100" bgcolor="#daf1ff" |[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#PlasmaTherm.2FSLR_Fluorine_Etcher SLR Fluorine ICP (PlasmaTherm)]
+
| width="100" bgcolor="#daf1ff" |[https://wiki.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#PlasmaTherm.2FSLR_Fluorine_Etcher SLR Fluorine ICP (PlasmaTherm)]
 
| width="120" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic 1)]]
 
| width="120" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br>(Panasonic 1)]]
 
| width="120" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic 2)]]
 
| width="120" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br>(Panasonic 2)]]
Line 22: Line 21:
 
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
 
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
 
| width="95" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
 
| width="95" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
| width="95" bgcolor="#daf1ff" |[[Plasma Clean (YES EcoClean)]]
+
| width="95" bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean (YES EcoClean)]]
 
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
 
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
 
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
 
| width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
Line 29: Line 28:
 
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
 
| width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]]
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Ag
+
! bgcolor="#d0e7ff" align="center" |Ag
|
 
|
 
 
|
 
|
 
|
 
|
Line 47: Line 44:
 
|
 
|
 
|
 
|
 
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Al
+
! bgcolor="#d0e7ff" align="center" |Al
|
 
 
|
 
|
 
|
 
|
Line 65: Line 62:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Au
+
! bgcolor="#d0e7ff" align="center" |Au
 
|
 
|
 
|
 
|
Line 83: Line 80:
 
|
 
|
 
|
 
|
  +
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|
 
|[https://www.nanotech.ucsb.edu/wiki/index.php/Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29 A]
 
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Cr
+
! bgcolor="#d0e7ff" align="center" |Cr
|
 
 
|
 
|
 
|
 
|
Line 103: Line 98:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Cu
+
! bgcolor="#d0e7ff" align="center" |Cu
|
 
|
 
 
|
 
|
 
|
 
|
Line 123: Line 116:
 
|
 
|
 
|
 
|
 
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |Ge
+
! bgcolor="#d0e7ff" align="center" |Ge
 
|
 
|
 
|
 
|
Line 138: Line 132:
 
|
 
|
 
|
 
|
 
|A
 
|
 
|
 
|A
 
|A
|
 
|
 
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Mo
+
! bgcolor="#d0e7ff" align="center" |Mo
|
 
|
 
 
|
 
|
 
|
 
|
Line 161: Line 152:
 
|
 
|
 
|
 
|
 
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |Ni
+
! bgcolor="#d0e7ff" align="center" |Ni
|
 
 
|
 
|
 
|
 
|
Line 181: Line 172:
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |Pt
+
! bgcolor="#d0e7ff" align="center" |Pt
|
 
 
|
 
|
 
|
 
|
Line 200: Line 190:
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |Ru
+
! bgcolor="#d0e7ff" align="center" |Ru
|
 
 
|
 
|
 
|
 
|
Line 217: Line 206:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Si
+
! bgcolor="#d0e7ff" align="center" |Si
|
 
 
|
 
|
 
|
 
|
Line 236: Line 224:
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (XeF2 Etcher)}}
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (XeF2 Etcher)}}
 
|
 
|
|
+
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |Ta
+
! bgcolor="#d0e7ff" align="center" |Ta
|
 
|
 
 
|
 
|
 
|
 
|
Line 256: Line 242:
 
|
 
|
 
|
 
|
 
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |Ti
+
! bgcolor="#d0e7ff" align="center" |Ti
|
 
 
|
 
|
 
|
 
|
Line 274: Line 260:
 
|
 
|
 
|
 
|
|
+
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |Al<sub>2</sub>O<sub>3</sub>
+
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub>
 
|
 
|
 
|
 
|
Line 283: Line 269:
 
|
 
|
 
|
 
|
 
|[https://wiki.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R]
|
 
|[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R]
 
|
 
 
|
 
|
 
|
 
|
Line 294: Line 278:
 
|
 
|
 
|
 
|
 
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub>
+
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub>
|
 
 
|
 
|
 
|
 
|
Line 312: Line 296:
 
|
 
|
 
|
 
|
|
+
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |AlGaAs
+
! bgcolor="#d0e7ff" align="center" |AlGaAs
|
 
 
|
 
|
 
|
 
|
Line 331: Line 314:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |AlGaN
+
! bgcolor="#d0e7ff" align="center" |AlGaN
|
 
 
|
 
|
 
|
 
|
Line 350: Line 332:
 
|
 
|
 
|
 
|
|
+
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |AlN
+
! bgcolor="#d0e7ff" align="center" |AlN
|
 
 
|
 
|
 
|
 
|
Line 369: Line 350:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |CdZnTe
+
! bgcolor="#d0e7ff" align="center" |CdZnTe
|
 
 
|{{rl|RIE Etching Recipes|CdZnTe Etch (RIE 2)}}
 
|{{rl|RIE Etching Recipes|CdZnTe Etch (RIE 2)}}
 
|
 
|
Line 388: Line 368:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |GaAs
+
! bgcolor="#d0e7ff" align="center" |GaAs
|
 
 
|
 
|
 
|
 
|
Line 407: Line 386:
 
|
 
|
 
|
 
|
|
+
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |GaN
+
! bgcolor="#d0e7ff" align="center" |GaN
|
 
 
|
 
|
 
|
 
|
Line 426: Line 404:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |GaSb
+
! bgcolor="#d0e7ff" align="center" |GaSb
|
 
 
|
 
|
 
|
 
|
Line 445: Line 422:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |HfO<sub>2</sub>
+
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub>
|
 
|
 
 
|
 
|
 
|
 
|
Line 465: Line 440:
 
|
 
|
 
|
 
|
 
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |InGaAlAs
+
! bgcolor="#d0e7ff" align="center" |InGaAlAs
|
 
 
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
 
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
 
|
 
|
Line 483: Line 458:
 
|
 
|
 
|
 
|
|
+
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |InGaAsP
+
! bgcolor="#d0e7ff" align="center" |InGaAsP
|
 
 
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
 
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
 
|
 
|
Line 502: Line 476:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |InP
+
! bgcolor="#d0e7ff" align="center" |InP
|
 
 
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
 
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}}
 
|
 
|
Line 521: Line 494:
 
|
 
|
 
|
 
|
  +
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}}
|
 
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |ITO
+
! bgcolor="#d0e7ff" align="center" |ITO
|
 
 
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}}
 
|{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}}
 
|
 
|
Line 540: Line 512:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
 
!Photoresist
 
!Photoresist
 
& ARC
 
& ARC
|
 
 
|
 
|
 
|A
 
|A
|[https://www.nanotech.ucsb.edu/wiki/index.php/RIE_Etching_Recipes#Photoresist_and_ARC R]
+
|[https://wiki.nanotech.ucsb.edu/wiki/index.php/RIE_Etching_Recipes#Photoresist_and_ARC R]
 
|
 
|
 
|
 
|
|[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_Etching R]
+
|[https://wiki.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_Etching R]
|[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_etching_2 R]
+
|[https://wiki.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_etching_2 R]
 
|
 
|
 
|A
 
|A
 
|A
 
|A
 
|A
Line 559: Line 531:
 
|
 
|
 
|
 
|
|
+
|A
|
 
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |SiC
+
! bgcolor="#d0e7ff" align="center" |SiC
|
 
 
|
 
|
 
|
 
|
Line 579: Line 549:
 
|
 
|
 
|
 
|
|
+
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |SiN
+
! bgcolor="#d0e7ff" align="center" |SiN
|
 
 
|
 
|
 
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}}
 
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}}
Line 598: Line 567:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |SiO<sub>2</sub>
+
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub>
|
 
 
|
 
|
 
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}}
 
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}}
 
|
 
|
 
|
 
|
  +
|{{rl|ICP Etching Recipes|SiO2 Etching (Fluorine ICP Etcher)}}
|A
 
 
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}}
 
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}}
 
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 2)}}
 
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 2)}}
Line 617: Line 585:
 
|
 
|
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}}
 
|{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}}
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |SiOxNy
+
! bgcolor="#d0e7ff" align="center" |SiOxNy
|
 
 
|
 
|
 
|
 
|
Line 636: Line 603:
 
|
 
|
 
|
 
|
|
+
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |Ta<sub>2</sub>O<sub>5</sub>
+
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub>
|
 
 
|
 
|
 
|
 
|
Line 655: Line 621:
 
|
 
|
 
|
 
|
|
+
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |TiN
+
! bgcolor="#d0e7ff" align="center" |TiN
|
 
|
 
 
|
 
|
 
|
 
|
Line 675: Line 639:
 
|
 
|
 
|
 
|
 
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |TiO<sub>2</sub>
+
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub>
|
 
|
 
 
|
 
|
 
|
 
|
Line 694: Line 657:
 
|
 
|
 
|
 
|
 
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |W-TiW
+
! bgcolor="#d0e7ff" align="center" |W-TiW
|
 
 
|
 
|
 
|
 
|
Line 712: Line 675:
 
|
 
|
 
|
 
|
|
+
|A
 
|- bgcolor="#eeffff"
 
|- bgcolor="#eeffff"
! align="center" bgcolor="#d0e7ff" |ZnO<sub>2</sub>
+
! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub>
|
 
|
 
 
|
 
|
 
|
 
|
Line 732: Line 693:
 
|
 
|
 
|
 
|
 
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |ZnS
+
! bgcolor="#d0e7ff" align="center" |ZnS
|
 
 
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
 
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
 
|
 
|
Line 750: Line 711:
 
|
 
|
 
|
 
|
|
+
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |ZnSe
+
! bgcolor="#d0e7ff" align="center" |ZnSe
|
 
 
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
 
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}}
 
|
 
|
Line 769: Line 729:
 
|
 
|
 
|
 
|
|
+
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |ZrO<sub>2</sub>
+
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub>
|
 
|
 
 
|
 
|
 
|
 
|
Line 789: Line 747:
 
|
 
|
 
|
 
|
 
|A
 
|-
 
|-
! align="center" bgcolor="#d0e7ff" |'''Material'''
+
! bgcolor="#d0e7ff" align="center" |'''Material'''
| bgcolor="#daf1ff" |[[RIE 1 (Custom)|RIE 1<br>(Retired)]]
 
 
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
 
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]]
 
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
 
| bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> (MRC)]]
Line 802: Line 760:
 
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
 
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br>(Technics PEII)]]
 
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
 
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Clean_.28Gasonics_2000.29|Plasma Clean<br>(Gasonics 2000)]]
| bgcolor="#daf1ff" |[[Plasma Clean (YES EcoClean)]]
+
| width="95" bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean (YES EcoClean)]]
 
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
 
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]]
 
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]
 
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]]

Revision as of 16:32, 4 February 2021

  • R = Recipe is available. Clicking this link will take you to the recipe.
  • A = Material is available for use, but no recipes are provided.
Dry Etching Recipes
RIE Etching ICP Etching Oxygen Plasma Systems Other Dry Etchers
Material RIE 2
(MRC)
RIE 3
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
SLR Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic 1)
ICP Etch 2
(Panasonic 2)
ICP-Etch
(Unaxis VLR)
Ashers
(Technics PEII)
Plasma Clean
(Gasonics 2000)
Plasma Clean (YES EcoClean) UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)
Ag A
Al A R R A
Au R
Cr A R A A
Cu A
Ge A A
Mo A
Ni R
Pt R
Ru A R A
Si R R R A
Ta A
Ti R A A
Al2O3 R A
Al2O3 (Sapphire) R A A
AlGaAs R R R A
AlGaN R A
AlN R A
CdZnTe R A
GaAs R R R R A
GaN R R R A
GaSb A R A
HfO2 A
InGaAlAs R R A
InGaAsP R R A
InP R A A R R
ITO R A
Photoresist

& ARC

A R R R A A A A
SiC R A A
SiN R R R A A
SiO2 R R R R R A
SiOxNy A A A
Ta2O5 A A
TiN A
TiO2 A
W-TiW R A A
ZnO2 A
ZnS R A
ZnSe R A
ZrO2 A
Material RIE 2
(MRC)
RIE 3
(MRC)
RIE 5
(PlasmaTherm)
DSEIII
(PlasmaTherm)
SLR Fluorine ICP (PlasmaTherm) ICP Etch 1
(Panasonic E626I)
ICP Etch 2
(Panasonic E640)
ICP-Etch
(Unaxis VLR)
Ashers
(Technics PEII)
Plasma Clean
(Gasonics 2000)
Plasma Clean (YES EcoClean) UV Ozone Reactor Plasma Activation
(EVG 810)
XeF2 Etch
(Xetch)
Vapor HF Etch
(uETCH)
CAIBE
(Oxford)