Direct-Write Lithography Recipes
Revision as of 23:24, 13 September 2020 by John d (talk | contribs) (John d moved page MLA150 Recipes to Maskless Aligner Recipes without leaving a redirect: higher level category)
Work In Progress This article is still under construction. It may contain factual errors. Content is subject to change. |
Photolithography Recipes for the Heidelberg MLA150.
Positive Resist (MLA150)
General notes: Hotplates used, filters, laser wavelengths, etc.
Resist | Spin Cond. | Bake | Thickness | Exposure Time | Focus Offset | PEB | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|
SPR955CM0.9 | 3 krpm/30” | 95°C/60” | ~ 0.9 um | AZ300MIF |
Negative Resist (MLA150)
General notes: Hotplates used, filters, laser wavelengths, etc.
Resist | Spin Cond. | Bake | Thickness | Exposure Time | Focus Offset | PEB | Flood | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|---|
AZ5214 | 6 krpm/30” | 95°C/60” | ~ 1.0 um | 60" | AZ300MIF | 60" |
|