Difference between revisions of "Direct-Write Lithography Recipes"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
(→‎Positive Resist (MLA150): added line-space for SPR 220-3)
Line 103: Line 103:
   
 
=== Negative Resist (MLA150) ===
 
=== Negative Resist (MLA150) ===
''We found that all the negative PR's we tested required the 375nm in order to be fully exposure with reasonable dose.''
+
''We found that all the negative PR's we tested required the 375nm in order to be fully exposed with reasonable dose/time.''
   
 
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;"
 
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;"

Revision as of 10:06, 12 December 2020

Maskless Aligner (Heidelberg MLA150)

Photolithography Recipes for the Heidelberg MLA150. All recipes were characterized on blank Silicon wafers. For different substrate coatings/materials, you will likely need to run a focus-exposure matrix ("series" exposure mode), using our params as a starting point.

These recipes use the same spin and bake params as our contact aligner and stepper recipes, using built-in hotplates on the photoresist spinner benches.

Positive Resist (MLA150)

We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work. Sub-micron features are possible. Overexposure is recommended to avoid stitching and horiz/vert discrepancies, compensate using CD Bias as described here.

Resist Spin Cond. Bake Thickness Laser (nm) Exposure Dose (mJ/cm2) DeFocus PEB Developer Developer Time Comments
AZ4110 4 krpm, 30s 95°C, 60s ~ 1.1 µm 405 240 5 none AZ400K:DI 1:4 50s Used MLA design (good for isolated lines 0.8-1um)
AZ4330 4 krpm, 30s 95°C, 60s ~ 3.3 µm 405 320 6 none AZ400K:DI 1:4 90s Used MLA design
AZ4620
SPR 220-3.0 2.5 krpm, 30s 115°C, 90s ~ 2.7 µm 405 325 - 4 115°C, 90s AZ300MIF 60s Used HIMT design. 0.6-0.9µm line/space.
SPR 955-CM0.9 3 krpm, 30s 95°C, 90s ~ 0.9 µm 405 250 - 7 110°C, 90s AZ300MIF 60s Used MLA design
THMR-3600HP 1.5 krpm, 45s;

250 rpm/s

100°C, 60s 0.430µm 405 180–220 -4 100°C, 60s AZ300MiF 20s ~0.4nm line/space:

lower dose for clear-field, higher dose for dark-field.

Negative Resist (MLA150)

We found that all the negative PR's we tested required the 375nm in order to be fully exposed with reasonable dose/time.

Resist Spin Cond. Bake Thickness Laser (nm) Exposure Dose (mJ/cm2) DeFocus PEB Flood Developer Developer Time Comments
AZ5214 6 krpm, 30s 95°C, 60s ~ 1.0 µm 375 35 - 5 110°C, 60s 60" AZ300MIF 60s Used UCSB design. Good for up to ~1.3um open line space.
AZnLOF2020 4 krpm, 30s 110°C, 60s ~ 2.1µm 375 340 - 3 110°C, 60s none AZ300MIF 90s Used UCSB design. Good for 2um open line space.
SU-8 2075 ~70µm 375 Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end.

Greyscale Lithography (MLA150)

AZ4620 is the manufacturer-recommended PR for greyscale litho.

Resist Spin Cond. Bake Thickness Exposure Dose (mJ/cm2) Focus Offset PEB Flood Developer Developer Time Comments
AZ4620 – krpm/30” 95°C, 60” 60" AZ300MIF 60s
  • TBD