== Heidelberg Instruments MLA150 ==
+
==[[Maskless Aligner (Heidelberg MLA150)]]==
Photolithography Recipes for the [[Maskless Aligner (Heidelberg MLA150)|Heidelberg MLA150]].  ''Description of litho params- different lasers available, greyscale etc.''
+
Photolithography Recipes for the [[Maskless Aligner (Heidelberg MLA150)|Heidelberg MLA150]].  All recipes were characterized on blank Silicon wafers. For different substrate coatings/materials, you will likely need to run a focus-exposure matrix ("series" exposure mode), using our params as a starting point.
  
=== Positive Resist (MLA150) ===
+
These recipes use the same spin and bake params as our contact aligner and stepper recipes, using built-in hotplates on the photoresist spinner benches.
''General notes: Hotplates used, filters, laser wavelengths, etc.''
 
  
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;"
+
'''''Any I-Line PR is usable''''', although we only characterized a select few below.  Run your own Focus-Exposure Matrix to characterize a new PR.
 +
 
 +
===Positive Resist (MLA150)===
 +
''We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work. Sub-micron features are possible.  Overexposure is recommended to avoid stitching and horiz/vert discrepancies, compensate using CD Bias [[MLA150 - Design Guidelines#High-Resolution Writing|as described here]].''
 +
 
 +
Note: calibrations done with the "HIMT design" will show higher dose, due to using only dark-field line/space patterns.
 +
 
 +
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
 
|- bgcolor="#D0E7FF"
 
|- bgcolor="#D0E7FF"
 
! width="100" |Resist
 
! width="100" |Resist
Line 16: Line 21:
 
! width="75" |Bake
 
! width="75" |Bake
 
! width="75" |Thickness
 
! width="75" |Thickness
! width="125" |Exposure Time
+
!Laser (nm)
! width="100" |Focus Offset
+
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>)
! width="75" |PEB
+
! width="100" |DeFocus
 +
! width="75" |PEB*
 
! width="100" |Developer
 
! width="100" |Developer
 
! width="125" |Developer Time
 
! width="125" |Developer Time
 
! width="300" |Comments
 
! width="300" |Comments
 
|-
 
|-
|SPR955CM0.9
+
|[[Media:AXP4000pb-Datasheet.pdf|AZ4110]]
|3 krpm/30”
+
|4 krpm, 30s
|95°C/60”
+
|95°C, 60s
|~ 0.9 um
+
|~ 1.1 µm
 +
|405
 +
|240
 +
|5
 +
|''none''
 +
|AZ400K:DI 1:4
 +
|50s
 +
|Used HIMT design (good for isolated lines 0.8-1um)
 +
|-
 +
 
 +
|[[Media:AXP4000pb-Datasheet.pdf|AZ4330]]
 +
|4 krpm, 30s
 +
|95°C, 60s
 +
|~ 3.3 µm
 +
|405
 +
|320
 +
|6
 +
|''none''
 +
|AZ400K:DI 1:4
 +
|90s
 +
|Used HIMT design
 +
|-
 +
|[[Media:AXP4000pb-Datasheet.pdf|AZ4620]]
 +
|
 +
|
 +
|
 
|
 
|
 
|
 
|
 
|
 
|
 +
|
 +
|
 +
|
 +
|
 +
|-
 +
|[[Media:SPR220-Positive-Resist-Datasheet.pdf|SPR 220-3.0]]
 +
|2.5 krpm, 30s
 +
|115°C, 90s
 +
|~ 2.7 µm
 +
|405
 +
|325
 +
| - 4
 +
|115°C, 90s
 +
|AZ300MIF
 +
|60s
 +
|Used HIMT design. 0.6-0.9µm line/space.
 +
|-
 +
|[[Media:SPR955-Positive-Resist-Datasheet.pdf|SPR 955-CM0.9]]
 +
|3 krpm, 30s
 +
|95°C, 90s
 +
|~ 0.9 µm
 +
|405
 +
|250
 +
| - 7
 +
|110°C, 90s
 
|AZ300MIF
 
|AZ300MIF
 +
|60s
 +
|Used HIMT design
 +
|-
 +
|[[Media:3600 D, D2v Spin Speed Curve.pdf|THMR-3600HP]]
 +
|1.5 krpm, 45s;
 +
250 rpm/s
 +
|100°C, 60s
 +
|0.430µm
 +
|405
 +
|180–220
 +
|<nowiki>-4</nowiki>
 +
|100°C, 60s
 +
|AZ300MiF
 +
|20s
 +
|~0.4nm line/space:
 +
 +
lower dose for clear-field, higher dose for dark-field.
 +
|-
 +
| colspan="11" |*PEB: Post-exposure bake
 +
|}
 +
 +
===Negative Resist (MLA150)===
 +
''We found that all the negative PR's we tested required the 375nm in order to be fully exposed with reasonable dose/time.''
 +
 +
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
 +
|- bgcolor="#D0E7FF"
 +
! width="100" |Resist
 +
! width="100" |Spin Cond.
 +
! width="75" |Bake
 +
! width="75" |Thickness
 +
!Laser (nm)
 +
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>)
 +
! width="100" |DeFocus
 +
! width="75" |PEB*
 +
! width="75" |Flood*
 +
! width="100" |Developer
 +
! width="125" |Developer Time
 +
! width="300" |Comments
 +
|-
 +
|[[Media:AZ5214-Negative-Resist-Datasheet.pdf|AZ5214]]
 +
|6 krpm, 30s
 +
|95°C, 60s
 +
|~ 1.0 µm
 +
|375
 +
|35
 +
| - 5
 +
|110°C, 60s
 +
|60"
 +
|AZ300MIF
 +
|60s
 +
|Used UCSB design. Good for up to ~1.3um open line space.
 +
|-
 +
|[[Media:AZnLOF2020-Negative-Resist-Datasheet.pdf|AZnLOF2020]]
 +
|4 krpm, 30s
 +
|110°C, 60s
 +
|~ 2.1µm
 +
|375
 +
|340
 +
| - 3
 +
|110°C, 60s
 +
|''none''
 +
|AZ300MIF
 +
|90s
 +
|Used UCSB design. Good for 2um open line space.
 +
|-
 +
|[[Media:SU-8-2075-revA.pdf|SU-8 2075]]
 +
|
 +
|
 +
|~70µm
 +
|375
 +
|
 +
|
 +
|
 +
|
 
|
 
|
| align="left" |
+
|
*??
+
|Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end.
*{{fl|SPR955CMstepperrecipe.pdf|See SPR955CM data file}}
+
|-
 +
| colspan="12" |*PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal, and requires Flood Exposure with the [[Contact Aligner (SUSS MA-6)|MA6]] or [[Suss Aligners (SUSS MJB-3)|MJB]] aligner afterwards, before developing.
 
|}
 
|}
=== Negative Resist (MLA150) ===
 
''General notes: Hotplates used, filters, laser wavelengths, etc.''
 
  
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;"
+
===Greyscale Lithography (MLA150)===
 +
''AZ4620 is the manufacturer-recommended PR for greyscale litho.''
 +
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
 
|- bgcolor="#D0E7FF"
 
|- bgcolor="#D0E7FF"
 
! width="100" |Resist
 
! width="100" |Resist
Line 45: Line 176:
 
! width="75" |Bake
 
! width="75" |Bake
 
! width="75" |Thickness
 
! width="75" |Thickness
! width="125" |Exposure Time
+
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>)
 
! width="100" |Focus Offset
 
! width="100" |Focus Offset
 
! width="75" |PEB
 
! width="75" |PEB
Line 53: Line 184:
 
! width="300" |Comments
 
! width="300" |Comments
 
|-
 
|-
|AZ5214
+
|[[Media:Az p4620 photoresist data package.pdf|AZ4620]]
|6 krpm/30”
+
|? krpm/30”
|95°C/60”
+
|95°C, 60”
|~ 1.0 um
+
|
 
|
 
|
 
|
 
|
Line 62: Line 193:
 
|60"
 
|60"
 
|AZ300MIF
 
|AZ300MIF
|60"
+
|60s
 
| align="left" |
 
| align="left" |
*???
+
*''TBD''
 
|}
 
|}

Latest revision as of 11:23, 1 December 2022

Maskless Aligner (Heidelberg MLA150)

Photolithography Recipes for the Heidelberg MLA150. All recipes were characterized on blank Silicon wafers. For different substrate coatings/materials, you will likely need to run a focus-exposure matrix ("series" exposure mode), using our params as a starting point.

These recipes use the same spin and bake params as our contact aligner and stepper recipes, using built-in hotplates on the photoresist spinner benches.

Any I-Line PR is usable, although we only characterized a select few below. Run your own Focus-Exposure Matrix to characterize a new PR.

Positive Resist (MLA150)

We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work. Sub-micron features are possible. Overexposure is recommended to avoid stitching and horiz/vert discrepancies, compensate using CD Bias as described here.

Note: calibrations done with the "HIMT design" will show higher dose, due to using only dark-field line/space patterns.

Resist Spin Cond. Bake Thickness Laser (nm) Exposure Dose (mJ/cm2) DeFocus PEB* Developer Developer Time Comments
AZ4110 4 krpm, 30s 95°C, 60s ~ 1.1 µm 405 240 5 none AZ400K:DI 1:4 50s Used HIMT design (good for isolated lines 0.8-1um)
AZ4330 4 krpm, 30s 95°C, 60s ~ 3.3 µm 405 320 6 none AZ400K:DI 1:4 90s Used HIMT design
AZ4620
SPR 220-3.0 2.5 krpm, 30s 115°C, 90s ~ 2.7 µm 405 325 - 4 115°C, 90s AZ300MIF 60s Used HIMT design. 0.6-0.9µm line/space.
SPR 955-CM0.9 3 krpm, 30s 95°C, 90s ~ 0.9 µm 405 250 - 7 110°C, 90s AZ300MIF 60s Used HIMT design
THMR-3600HP 1.5 krpm, 45s;

250 rpm/s

100°C, 60s 0.430µm 405 180–220 -4 100°C, 60s AZ300MiF 20s ~0.4nm line/space:

lower dose for clear-field, higher dose for dark-field.

*PEB: Post-exposure bake

Negative Resist (MLA150)

We found that all the negative PR's we tested required the 375nm in order to be fully exposed with reasonable dose/time.

Resist Spin Cond. Bake Thickness Laser (nm) Exposure Dose (mJ/cm2) DeFocus PEB* Flood* Developer Developer Time Comments
AZ5214 6 krpm, 30s 95°C, 60s ~ 1.0 µm 375 35 - 5 110°C, 60s 60" AZ300MIF 60s Used UCSB design. Good for up to ~1.3um open line space.
AZnLOF2020 4 krpm, 30s 110°C, 60s ~ 2.1µm 375 340 - 3 110°C, 60s none AZ300MIF 90s Used UCSB design. Good for 2um open line space.
SU-8 2075 ~70µm 375 Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end.
*PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal, and requires Flood Exposure with the MA6 or MJB aligner afterwards, before developing.

Greyscale Lithography (MLA150)

AZ4620 is the manufacturer-recommended PR for greyscale litho.

Resist Spin Cond. Bake Thickness Exposure Dose (mJ/cm2) Focus Offset PEB Flood Developer Developer Time Comments
AZ4620 ? krpm/30” 95°C, 60” 60" AZ300MIF 60s
  • TBD