==SiO<sub>2</sub> deposition (PECVD #1)== |
==SiO<sub>2</sub> deposition (PECVD #1)== |
||
− | * SiO<sub>2</sub> [PECVD 1] Standard Recipe |
+ | *[https://docs.google.com/spreadsheets/d/1uqpg3sirsRbXdTFlxZ6_k3t0ovP0MtpFtICjpH0-prs/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>] |
− | * |
+ | *[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=0 SiO<sub>2</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>] |
− | * |
+ | *[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=1503619544 SiO<sub>2</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier |
==SiN deposition (PECVD #1)== |
==SiN deposition (PECVD #1)== |
||
− | * Si<sub>3</sub>N<sub>4</sub> [PECVD 1] Standard Recipe |
+ | *[https://docs.google.com/spreadsheets/d/1DGU745SeunYz4sLs1LpGKbtOYX-tQyBHEvVYcMxHRKE/edit#gid= Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>] |
− | * |
+ | *[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=98787450 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>] |
− | * |
+ | *[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=604790654 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier |
==Low Stress Si<sub>3</sub>N<sub>4</sub> (PECVD#1)== |
==Low Stress Si<sub>3</sub>N<sub>4</sub> (PECVD#1)== |
||
− | * Low Stress Si<sub>3</sub>N<sub>4</sub> [PECVD 1] Standard Recipe |
+ | *[https://wiki.nanotech.ucsb.edu/wiki/images/4/4a/New_PECVD1-LS_SIN-Turner05recipe_2014_LS_SIN_recipe.pdf Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>] |
− | * |
+ | *[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=1515630363 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>] |
− | * |
+ | *[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=934830479 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - 2021-10 and earlier |
==SiO<sub>x</sub>N<sub>y</sub> deposition (PECVD #1)== |
==SiO<sub>x</sub>N<sub>y</sub> deposition (PECVD #1)== |
||
Line 37: | Line 37: | ||
#Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. ) |
#Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. ) |
||
#Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning. |
#Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning. |
||
+ | # |
||
+ | |||
+ | {| class="wikitable" |
||
+ | |+Table of Cleaning Times |
||
+ | !Film Dep'd |
||
+ | !Cleaning Time |
||
+ | |- |
||
+ | |SiO<sub>2</sub> |
||
+ | |TBD |
||
+ | |- |
||
+ | |Si<sub>3</sub>N<sub>4</sub> |
||
+ | |TBD |
||
+ | |- |
||
+ | |SiOxNy |
||
+ | |Same as XYZ |
||
+ | |} |
||
+ | |||
+ | # |
||
===[https://wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"]=== |
===[https://wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"]=== |
||
Line 46: | Line 64: | ||
==SiO<sub>2</sub> deposition (PECVD #2)== |
==SiO<sub>2</sub> deposition (PECVD #2)== |
||
− | SiO<sub>2</sub> [PECVD 2] Standard Recipe |
||
− | [https://docs.google.com/spreadsheets/d/ |
+ | * [https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 2] Standard Recipe</nowiki>] - "''STD SiO2''" |
⚫ | |||
⚫ | |||
⚫ | |||
==SiN deposition (PECVD #2)== |
==SiN deposition (PECVD #2)== |
||
⚫ | |||
− | ===Standard Recipe=== |
||
− | Si<sub>3</sub>N<sub>4</sub> [PECVD 2] |
+ | * [https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=773875841 Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>] |
⚫ | |||
− | |||
− | ===Present Data=== |
||
⚫ | |||
− | |||
− | ===Historical Data=== |
||
⚫ | |||
==Low-Stress SiN deposition (PECVD #2)== |
==Low-Stress SiN deposition (PECVD #2)== |
||
''Low-Stress SilIcon Nitride, Si<sub>3</sub>N<sub>4</sub> (< 100 MPa)'' |
''Low-Stress SilIcon Nitride, Si<sub>3</sub>N<sub>4</sub> (< 100 MPa)'' |
||
− | * Low Stress Si<sub>3</sub>N<sub>4</sub> [PECVD 2] Standard Recipe |
+ | *[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Standard Recipe</nowiki>] - "''LSNitride2''" |
+ | *** ''Old Versions of the recipe:'' |
||
⚫ | |||
+ | **** [https://wiki.nanotech.ucsb.edu/wiki/images/a/a5/New_AdvPECVD-LS_Nitride2_300C_standard_recipe_LS_Nitride2_standard_recipe.pdf LS Nitride2 Standard Recipe 2014-5/9/2018] |
||
⚫ | |||
+ | **** [https://wiki.nanotech.ucsb.edu/wiki/images/0/01/STD_LSNitride2_5-9-18.pdf STD LSNitride2 5/9/2018] |
||
⚫ | |||
⚫ | |||
==Amorphous-Si deposition (PECVD #2)== |
==Amorphous-Si deposition (PECVD #2)== |
||
Line 106: | Line 122: | ||
The system currently has Deuterated Silane (SiD<sub>4</sub>) installed - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. |
The system currently has Deuterated Silane (SiD<sub>4</sub>) installed - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. |
||
− | ===[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948 ICP-PECVD Plots]=== |
+ | ===[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948 ICP-PECVD Plots] - TBD=== |
==Low Deposition Rate SiO<sub>2</sub> [ICP-PECVD]== |
==Low Deposition Rate SiO<sub>2</sub> [ICP-PECVD]== |
||
⚫ | |||
− | ===Standard Recipe=== |
||
− | Low Deposition Rate SiO<sub>2</sub> [ICP-PECVD] |
+ | * [https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=0 Low Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>] |
⚫ | |||
− | |||
− | ===Present Data=== |
||
⚫ | |||
− | |||
− | ===Historical Data=== |
||
⚫ | |||
==High Deposition Rate SiO<sub>2</sub> [ICP-PECVD]== |
==High Deposition Rate SiO<sub>2</sub> [ICP-PECVD]== |
||
⚫ | |||
− | ===Standard Recipe=== |
||
− | High Deposition Rate SiO<sub>2</sub> [ICP-PECVD] |
+ | * [https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 High Deposition Rate SiO<sub>2</sub><nowiki> [ICP-PECVD] Present Data</nowiki>] |
⚫ | |||
− | ===Present Data=== |
||
⚫ | |||
− | |||
− | ===Historical Data=== |
||
⚫ | |||
==Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]== |
==Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]== |
||
⚫ | |||
− | ===Standard Recipe=== |
||
− | Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD] |
+ | * [https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Current Process Control Data</nowiki>] |
⚫ | |||
− | |||
− | ===Present Data=== |
||
⚫ | |||
− | |||
− | ===Historical Data=== |
||
⚫ | |||
==Low Stress Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]== |
==Low Stress Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]== |
||
⚫ | |||
− | ===Standard Recipe=== |
||
− | Low Stress Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD] |
+ | * [https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Current Process Control Data</nowiki>] |
+ | * [https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1024532473 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Historical Data</nowiki>] - before Oct. 2021 |
||
− | ===Present Data=== |
||
⚫ | |||
− | |||
− | ===Historical Data=== |
||
⚫ | |||
==Standard Cleaning Procedure [ICP-PECVD]== |
==Standard Cleaning Procedure [ICP-PECVD]== |
||
You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the [[ICP-PECVD (Unaxis VLR)#Documentation|Operating Procedure on the Unaxis Tool Page]] for details. |
You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the [[ICP-PECVD (Unaxis VLR)#Documentation|Operating Procedure on the Unaxis Tool Page]] for details. |
||
Line 157: | Line 155: | ||
===Standard Clean Recipe=== |
===Standard Clean Recipe=== |
||
+ | ''To Be Added'' |
||
+ | |||
=[[Ion Beam Deposition (Veeco NEXUS)]]= |
=[[Ion Beam Deposition (Veeco NEXUS)]]= |
||
Revision as of 23:49, 15 December 2021
NEW data templates - Demis 2021-12-15
Back to Vacuum Deposition Recipes
PECVD 1 (PlasmaTherm 790)
PECVD 1 Plots - SiO2, SiN and Particulate Count
SiO2 deposition (PECVD #1)
- SiO2 [PECVD 1] Standard Recipe
- SiO2 [PECVD 1] Current Process Control Data
- SiO2 [PECVD 1] Historical Data - Oct. 2021 and earlier
SiN deposition (PECVD #1)
- Si3N4 [PECVD 1] Standard Recipe
- Si3N4 [PECVD 1] Current Process Control Data
- Si3N4 [PECVD 1] Historical Data - Oct. 2021 and earlier
Low Stress Si3N4 (PECVD#1)
- Low Stress Si3N4 [PECVD 1] Standard Recipe
- Low Stress Si3N4 [PECVD 1] Current Process Control Data
- Low Stress Si3N4 [PECVD 1] Historical Data - 2021-10 and earlier
SiOxNy deposition (PECVD #1)
Standard Cleaning Procedure (PECVD #1)
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
- Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
- Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.
Film Dep'd | Cleaning Time |
---|---|
SiO2 | TBD |
Si3N4 | TBD |
SiOxNy | Same as XYZ |
Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.
PECVD 2 (Advanced Vacuum)
PECVD 2 Plots
SiO2 deposition (PECVD #2)
- SiO2 [PECVD 2] Standard Recipe - "STD SiO2"
- SiO2 [PECVD 2] Current Process Control Data
- SiO2 [PECVD 2] Historical Data - Before Oct. 2021
SiN deposition (PECVD #2)
- Si3N4 [PECVD 2] Standard Recipe - "Nitride2"
- Si3N4 [PECVD 2] Current Process Control Data
- Si3N4 [PECVD 2] Historical Data - Before Oct. 2021
Low-Stress SiN deposition (PECVD #2)
Low-Stress SilIcon Nitride, Si3N4 (< 100 MPa)
- Low Stress Si3N4 [PECVD 2] Standard Recipe - "LSNitride2"
- Old Versions of the recipe:
- Low Stress Si3N4 [PECVD 2] Current Process Control Data
- Low Stress Si3N4 [PECVD 2] Historical Data - Before Oct. 2021
Amorphous-Si deposition (PECVD #2)
Standard Cleaning Procedure (PECVD #2)
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
- (If >29min dep time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again.
- Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.
Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.
Clean Times (PECVD#2)
Film Deposited | Cleaning Time (Dry) |
---|---|
SiO2 | 1 min. clean for every 1 min. deposition |
Si3N4 | 1 min. clean for every 7 min of deposition |
If > 29min total dep time
(Season + Dep) |
Wet Clean the Upper Lid/Chamber
DI water then Isopropyl Alcohol on chamber wall & portholes |
ICP-PECVD (Unaxis VLR)
2020-02: New recipes have been characterized for low particulate count and repeatability. Only staff-supplied recipes are allowed in the tool. Please follow the new procedures to ensure low particle counts in the chamber.
The system currently has Deuterated Silane (SiD4) installed - identical to the regular Silicon precursor SiH4, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights.
ICP-PECVD Plots - TBD
Low Deposition Rate SiO2 [ICP-PECVD]
- Low Deposition Rate SiO2 [ICP-PECVD] - Standard Recipe - "SiO2 LDR 250C"
- Low Deposition Rate SiO2 [ICP-PECVD] - Current Process Control Data
- Low Deposition Rate SiO2 [ICP-PECVD] - Historical Data - before Oct. 2021
High Deposition Rate SiO2 [ICP-PECVD]
- High Deposition Rate SiO2 [ICP-PECVD] Standard Recipe - "SiO2 HDR 250C"
- High Deposition Rate SiO2 [ICP-PECVD] Present Data
- High Deposition Rate SiO2 [ICP-PECVD] Historical Data
Si3N4 [ICP-PECVD]
- Si3N4 [ICP-PECVD] Standard Recipe - "SiN 250C"
- Si3N4 [ICP-PECVD] Current Process Control Data
- Si3N4 [ICP-PECVD] Historical Data - before Oct. 2021
Low Stress Si3N4 [ICP-PECVD]
- Low Stress Si3N4 [ICP-PECVD] Standard Recipe - "SiN Low Stress 250C"
- Low Stress Si3N4 [ICP-PECVD] Current Process Control Data
- Low Stress Si3N4 [ICP-PECVD] Historical Data - before Oct. 2021
Standard Cleaning Procedure [ICP-PECVD]
You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.
- SiNx etches at 20nm/min
- SiO2 etches at 40nm/min
Standard Clean Recipe
To Be Added
Ion Beam Deposition (Veeco NEXUS)
IBD Plots
SiO2 [IBD]
Standard Recipe
SiO2 [IBD] Standard Recipe
Present Data
Historical Data
Si3N4 [IBD]
Standard Recipe
Si3N4 [IBD] Standard Recipe
Present Data
Historical Data
Ta2O5 [IBD]
Standard Recipe
Ta2O5 [IBD] Standard Recipe
Present Data
Historical Data
Al2O3 [IBD]
Standard Recipe
Al2O3 [IBD] Standard Recipe
Present Data
Historical Data
TiO2 [IBD]
Standard Recipe
TiO2 [IBD] Standard Recipe
Present Data
Historical Data
Standard Cleaning Procedure [ICP-PECVD]
You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.
- SiNx etches at 20nm/min
- SiO2 etches at 40nm/min
Standard Clean Recipe