== Oxford FlexAL Chamber #1: Metals == |
== Oxford FlexAL Chamber #1: Metals == |
||
+ | '''Maximum 30nm deposition thickness!''' (ask [[Brian Lingg|Tool Supervisor]] if needed.) |
||
+ | ''Note that Plasma-based (indicated by asterisk eg.'' N* ''or'' O*'') recipes run nearly 2x faster than H2O/thermal recipes due to faster reaction rate, thus shorter cycling.'' |
||
=== Pt deposition (ALD CHAMBER 1) === |
=== Pt deposition (ALD CHAMBER 1) === |
||
*Recipe name: '''''Ch1_TMCpPt+O3-300C''''' |
*Recipe name: '''''Ch1_TMCpPt+O3-300C''''' |
||
− | *Pt deposition rate ~ 0.5-0. |
+ | **Pt deposition rate ~ 0.5-0.6 A/cyc |
⚫ | |||
− | *recipe utilizes the ozone generator which must be first set to the following conditions: |
+ | **recipe utilizes the ozone generator which must be first set to the following conditions: |
⚫ | |||
− | **O<sub> |
+ | ***O<sub>2</sub> flow = 250sccm |
⚫ | |||
⚫ | |||
+ | **300°C deposition |
||
+ | *Recipe name: '''''CH1-TMCpPt+250W/O*-300C''''' |
||
+ | **Uses Oxygen plasma |
||
+ | **300°C deposition |
||
=== Ru deposition (ALD CHAMBER 1) === |
=== Ru deposition (ALD CHAMBER 1) === |
||
Line 16: | Line 22: | ||
* Ru deposition rate ~ 0.6-0.7A/cyc. |
* Ru deposition rate ~ 0.6-0.7A/cyc. |
||
* Conductivity data: (to be added) |
* Conductivity data: (to be added) |
||
+ | * 300°C, O2 gas reaction |
||
=== ZnO Deposition (ALD Chamber 1) === |
=== ZnO Deposition (ALD Chamber 1) === |
||
− | + | ''Conductive film.'' |
|
* Recipe name: '''''Ch1_DEZ+H2O-200C''''' |
* Recipe name: '''''Ch1_DEZ+H2O-200C''''' |
||
− | * ZnO deposition rate ≈ |
+ | * ZnO deposition rate ≈ 1.6 A/cycle |
*resistivity ≈ ''TBA'' |
*resistivity ≈ ''TBA'' |
||
+ | *200°C Deposition, Water reaction |
||
=== ZnO:Al deposition (ALD CHAMBER 1) === |
=== ZnO:Al deposition (ALD CHAMBER 1) === |
||
Line 32: | Line 40: | ||
== Oxford FlexAL Chamber #3: Dielectrics == |
== Oxford FlexAL Chamber #3: Dielectrics == |
||
+ | '''Maximum 30nm deposition thickness!''' (ask [[Brian Lingg|Tool Supervisor]] if needed.) |
||
===Al{{sub|2}}O{{sub|3}} deposition (ALD CHAMBER 3)=== |
===Al{{sub|2}}O{{sub|3}} deposition (ALD CHAMBER 3)=== |
||
− | *Recipe name: ''''' |
+ | *Recipe name: '''''CH3-TMA+H2O-<u>300C</u>''''' |
− | *Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1A/cyc |
+ | **Al<sub>2</sub>O<sub>3</sub> deposition rate ~ 1A/cyc |
+ | **300°C Dep., Water reaction |
||
+ | **This is considered the standard recipe for ALD |
||
+ | **Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C |
||
+ | *Recipe Name: '''''CH3-TMA+250W/O*-300C''''' |
||
+ | **Similar deposition rate |
||
+ | **Oxygen Plasma reaction instead of H2O |
||
+ | **Lower carbon content, approx. <u>1.5–2x faster deposition rate.</u> |
||
+ | **Temperature variations: 300°C (std.), 200°C, 120°C |
||
+ | *Recipe Name: '''''CH3-TMA+O3/200mT-300C''''' |
||
+ | **Similar dep. rate |
||
+ | **Ozone (O<sub>3</sub>) reactant, experimental |
||
===AlN deposition (ALD CHAMBER 3)=== |
===AlN deposition (ALD CHAMBER 3)=== |
||
− | *Recipe name: ''''' |
+ | *Recipe name: '''''CH3-TMA+100W/N*-300C''''' |
− | *AlN deposition rate ~ t.b.d. |
+ | **AlN deposition rate ~ t.b.d. |
− | * |
+ | **Recipe utilizes a N* plasma @ 100W, 20mTorr pressure. |
+ | **Temperature Variations: 300°C Dep. (std.), 200*C, 120°C |
||
+ | **Power variations: 300W, 400W (at 300°C) |
||
+ | **Nitrogen/Hydrogen variations: "30N*/30H*" at 200*C and 300°C |
||
===HfO{{sub|2}} deposition (ALD CHAMBER 3)=== |
===HfO{{sub|2}} deposition (ALD CHAMBER 3)=== |
||
− | *Recipe name: ''''' |
+ | *Recipe name: '''''CH3-TEMAH+H2O-300C''''' |
− | *HfO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
+ | **HfO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
− | *Note: deposition shows significant parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
+ | **Note: deposition shows significant parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
+ | **Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C |
||
+ | *Recipe name: '''''CH3-TEMAH+250W/O*-300C''''' |
||
+ | **Uses Oxygen plasma reactant instead of H<sub>2</sub>O |
||
+ | *Recipe name: '''''CH3-TEMAH+O3/100mT-300C''''' |
||
+ | **Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O |
||
===SiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
===SiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
||
− | *Recipe name: ''''' |
+ | *Recipe name: '''''CH3-TDMAS+250W/O*-300C''''' |
− | *SiO<sub>2</sub> deposition rate ~ 0.7-0.8A/cyc |
+ | **SiO<sub>2</sub> deposition rate ~ 0.7-0.8A/cyc |
− | * |
+ | **Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp. |
+ | **Temperature variations: 300*C (std.), 250°C, 230°C, 200°C, 150°C, 120°C |
||
+ | *Recipe name: '''''CH3-TDMAS+O3/200mT-300C''''' |
||
+ | **Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O |
||
===ZrO{{sub|2}} deposition (ALD CHAMBER 3)=== |
===ZrO{{sub|2}} deposition (ALD CHAMBER 3)=== |
||
− | *Recipe name: ''''' |
+ | *Recipe name: '''''CH3-TEMAZ+H2O-300C''''' |
− | *ZrO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
+ | **ZrO<sub>2</sub> deposition rate ~ 0.9-1.0A/cyc |
− | * |
+ | **Not directly characterized since results are basically the same as the HfO<sub>2</sub> process above. |
+ | **Temperature variations: 300°C (std.), 200°C |
||
− | *as for the HfO<sub>2</sub> process, deposition will exhibit significant parasitic growth unless long H<sub>2</sub>O purge/pump cycles are in place. |
||
+ | *Recipe name: '''''CH3-TEMAZ+250W/O*-300C''''' |
||
+ | **Uses Oxygen plasma reactant instead of H<sub>2</sub>O |
||
+ | *Recipe name: '''''CH3-TEMAZ+O3/100mT-300C''''' |
||
+ | **Uses Ozone (O<sub>3</sub>) for reactant instead of H<sub>2</sub>O |
||
===TiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
===TiO{{sub|2}} deposition (ALD CHAMBER 3)=== |
||
− | *Recipe name: ''''' |
+ | *Recipe name: '''''CH3-TDMAT+H2O-300C''''' |
− | *TiO |
+ | **TiO<sub>2</sub> deposition rate ~ 0.6A/cyc |
− | *Note: deposition shows parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
+ | **Note: deposition shows parasitic growth (via CVD channel) if H<sub>2</sub>O purge/pump times are not sufficient. |
+ | **Temperature variations: 300°C (std.), 200°C, 120*C |
||
+ | *Recipe name: '''''CH3-TDMAT+250W/O*-300C''''' |
||
+ | **Uses Oxygen plasma reactant instead of H<sub>2</sub>O |
||
===TiN deposition (ALD CHAMBER 3)=== |
===TiN deposition (ALD CHAMBER 3)=== |
||
− | *Recipe name: ''''' |
+ | *Recipe name: '''''CH3-TDMAT+400W/12N*/4H*-300C''''' |
− | *TiN deposition rate ~ 0.7A/cyc |
+ | **TiN deposition rate ~ 0.7A/cyc |
− | *Conductivity data: (to be added |
+ | **Conductivity data: (to be added) |
+ | **Uses Plasma of N2 & H2 gases. |
||
+ | **Temperatures: 300°C (std.), 200°C |
||
+ | *Recipe name: '''''CH3-TDMAT+100W/N*-300C''''' |
||
+ | **Uses Plasma of N2 only |
||
+ | **Temperatures: 300°C (std.), 200°C |
||
+ | *Recipe name: '''''CH3-TDMAT+100W/NH3*-300C''''' |
||
+ | **Uses Plasma of NH<sub>3</sub> only |
||
+ | **Temperatures: 300°C (std.), 200°C |
Revision as of 07:46, 26 February 2021
Back to Vacuum Deposition Recipes.
Atomic Layer Deposition (Oxford FlexAL)
Oxford FlexAL Chamber #1: Metals
Maximum 30nm deposition thickness! (ask Tool Supervisor if needed.)
Note that Plasma-based (indicated by asterisk eg. N* or O*) recipes run nearly 2x faster than H2O/thermal recipes due to faster reaction rate, thus shorter cycling.
Pt deposition (ALD CHAMBER 1)
- Recipe name: Ch1_TMCpPt+O3-300C
- Pt deposition rate ~ 0.5-0.6 A/cyc
- Conductivity data: (to be added)
- recipe utilizes the ozone generator which must be first set to the following conditions:
- O2 flow = 250sccm
- O3 concentration = 15 wt%
- 300°C deposition
- Recipe name: CH1-TMCpPt+250W/O*-300C
- Uses Oxygen plasma
- 300°C deposition
Ru deposition (ALD CHAMBER 1)
- Recipe name: Ch1_Ex03Ru[HPbub]+O2-300C
- Ru deposition rate ~ 0.6-0.7A/cyc.
- Conductivity data: (to be added)
- 300°C, O2 gas reaction
ZnO Deposition (ALD Chamber 1)
Conductive film.
- Recipe name: Ch1_DEZ+H2O-200C
- ZnO deposition rate ≈ 1.6 A/cycle
- resistivity ≈ TBA
- 200°C Deposition, Water reaction
ZnO:Al deposition (ALD CHAMBER 1)
Al-Doped ZnO for variable resisitivity.
- Recipe name: Ch1_DEZ/TMA+H2O-200C
- The recipe has TWO loops. The Outer loop determines final thickness. The Inner loop determines how much AlOx is doped into the film. Note that each full (outer-loop) cycle takes a long time due to this double-loop structure.
- Al dose fraction = 5% for lowest resistivity
- ZnO deposition rate ~ 1.7A/cyc
- resistivity ~ 4200uOhm.cm (390A film)
Oxford FlexAL Chamber #3: Dielectrics
Maximum 30nm deposition thickness! (ask Tool Supervisor if needed.)
Al2O3 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TMA+H2O-300C
- Al2O3 deposition rate ~ 1A/cyc
- 300°C Dep., Water reaction
- This is considered the standard recipe for ALD
- Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
- Recipe Name: CH3-TMA+250W/O*-300C
- Similar deposition rate
- Oxygen Plasma reaction instead of H2O
- Lower carbon content, approx. 1.5–2x faster deposition rate.
- Temperature variations: 300°C (std.), 200°C, 120°C
- Recipe Name: CH3-TMA+O3/200mT-300C
- Similar dep. rate
- Ozone (O3) reactant, experimental
AlN deposition (ALD CHAMBER 3)
- Recipe name: CH3-TMA+100W/N*-300C
- AlN deposition rate ~ t.b.d.
- Recipe utilizes a N* plasma @ 100W, 20mTorr pressure.
- Temperature Variations: 300°C Dep. (std.), 200*C, 120°C
- Power variations: 300W, 400W (at 300°C)
- Nitrogen/Hydrogen variations: "30N*/30H*" at 200*C and 300°C
HfO2 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TEMAH+H2O-300C
- HfO2 deposition rate ~ 0.9-1.0A/cyc
- Note: deposition shows significant parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
- Temperature variations: 300°C (std.), 250°C, 200°C, 150°C, 120°C
- Recipe name: CH3-TEMAH+250W/O*-300C
- Uses Oxygen plasma reactant instead of H2O
- Recipe name: CH3-TEMAH+O3/100mT-300C
- Uses Ozone (O3) for reactant instead of H2O
SiO2 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TDMAS+250W/O*-300C
- SiO2 deposition rate ~ 0.7-0.8A/cyc
- Recipe utilizes an O* plasma @ 250W, 5mTorr pressure, 300°C Temp.
- Temperature variations: 300*C (std.), 250°C, 230°C, 200°C, 150°C, 120°C
- Recipe name: CH3-TDMAS+O3/200mT-300C
- Uses Ozone (O3) for reactant instead of H2O
ZrO2 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TEMAZ+H2O-300C
- ZrO2 deposition rate ~ 0.9-1.0A/cyc
- Not directly characterized since results are basically the same as the HfO2 process above.
- Temperature variations: 300°C (std.), 200°C
- Recipe name: CH3-TEMAZ+250W/O*-300C
- Uses Oxygen plasma reactant instead of H2O
- Recipe name: CH3-TEMAZ+O3/100mT-300C
- Uses Ozone (O3) for reactant instead of H2O
TiO2 deposition (ALD CHAMBER 3)
- Recipe name: CH3-TDMAT+H2O-300C
- TiO2 deposition rate ~ 0.6A/cyc
- Note: deposition shows parasitic growth (via CVD channel) if H2O purge/pump times are not sufficient.
- Temperature variations: 300°C (std.), 200°C, 120*C
- Recipe name: CH3-TDMAT+250W/O*-300C
- Uses Oxygen plasma reactant instead of H2O
TiN deposition (ALD CHAMBER 3)
- Recipe name: CH3-TDMAT+400W/12N*/4H*-300C
- TiN deposition rate ~ 0.7A/cyc
- Conductivity data: (to be added)
- Uses Plasma of N2 & H2 gases.
- Temperatures: 300°C (std.), 200°C
- Recipe name: CH3-TDMAT+100W/N*-300C
- Uses Plasma of N2 only
- Temperatures: 300°C (std.), 200°C
- Recipe name: CH3-TDMAT+100W/NH3*-300C
- Uses Plasma of NH3 only
- Temperatures: 300°C (std.), 200°C